Super-hydrophilic modification method and application of hollow fiber organic membrane
By super-hydrophilic modification of the hollow fiber organic membrane, covering manganese oxide armor and using the chlorine resistance of metal oxides, the pollution and corrosion problems of polymer ultrafiltration membranes when treating algae water are extended The membrane life and purification efficiency are improved, achieving a low-carbon and environmentally friendly filtration and backflushing process.
Patent Information
- Application Number
- CN202411253849.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The existing polymer ultrafiltration membranes are prone to membrane contamination and chemical corrosion during the treatment of algae-containing water, resulting in a shortening of the membrane service life and affecting the efficiency of drinking water purification and wastewater treatment.
Using the super hydrophilic modification method of hollow fiber organic film, the hydrophilicity and anti-adhesion properties of the film are improved by coating manganese oxide armor, and the anti-chlorine properties of metal oxides are used to chemically clean using sodium hypochlorite to extend the film. life.
It effectively reduces the membrane pollution rate and irreversible pollution degree, improves the dynamic pollution resistance and life of the membrane, and realizes a low-carbon and environmentally friendly filtration and backflushing process.
Smart Images

Figure CN118925512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of drinking water purification and wastewater pollution control, and specifically relates to a super-hydrophilic modification method and application of a hollow fiber organic membrane. Background Art
[0002] The massive growth of algae caused by eutrophication accelerates the corrosion of pipes and interferes with the coagulation and filtration processes. In addition, algae-derived metabolites and disinfection by-product precursors threaten public health and are a major challenge in the process of water environment protection and governance. Ultrafiltration membrane technology, based on the size exclusion principle and relatively low operating energy consumption, has become one of the most widely used drinking water deep treatment technologies. However, the serious membrane fouling caused by ultrafiltration treatment of algae-containing water restricts the further promotion of ultrafiltration technology. At the same time, chlorine is widely used as a pre-oxidant, membrane cleaning agent and disinfectant in actual engineering. However, cleaning with sodium hypochlorite will destroy the organic membrane structure and further reduce the service life of the membrane.
[0003] Hollow fiber membranes have the advantages of high packing density per unit volume, large filtration area, small footprint and relatively low cost, making them the fastest growing, largest scale and highest value-added new type of membrane technology product in the separation membrane field. Summary of the invention
[0004] The purpose of the present invention is to solve the membrane pollution and chemical agent corrosion problems of polymer ultrafiltration membranes in existing practical operation, and to provide a super-hydrophilic modification method and application of hollow fiber organic membranes.
[0005] The present invention provides a method and application of super-hydrophilic modification of a hollow fiber organic membrane. Manganese oxide tends to combine with water and forms hydroxyl groups on the surface, so the hydrophilicity is improved. Based on this characteristic, the present invention improves the hydrophilicity of the membrane surface by coating manganese oxide armor, which can reduce the membrane contamination rate and the irreversible contamination degree, and increase the anti-adhesion performance of the membrane surface. At the same time, by utilizing the anti-chlorine property of the metal oxide, the structural damage of the polymer hollow fiber membrane can be effectively avoided when chemical cleaning is performed with sodium hypochlorite, and the life of the membrane component is extended, laying a foundation for its research in the field of drinking water purification and wastewater pollution control.
[0006] A method for super-hydrophilic modification of a hollow fiber organic membrane is specifically completed by the following steps:
[0007] 1. Pretreatment of organic membrane:
[0008] The hollow fiber ultrafiltration membrane is rinsed with deionized water to obtain a pretreated hollow fiber ultrafiltration membrane;
[0009] 2. Prepare the manganese oxide colloidal particle solution:
[0010] First, add potassium permanganate to deionized water, stir evenly and continuously introduce N 2 Purging was performed to obtain a potassium permanganate solution; then 2 Under the protection of the atmosphere, a sodium thiosulfate solution is dripped into the potassium permanganate solution while stirring; after the dripping is completed, brown manganese oxide colloidal particles are formed, and stirring is continued for a period of time to obtain a manganese oxide colloidal particle solution, which is stored in the dark at 4°C;
[0011] 3. Introducing the base layer on the surface of the hollow fiber ultrafiltration membrane:
[0012] The manganese oxide colloidal particle solution is assembled onto the surface of the pretreated hollow fiber ultrafiltration membrane by filtering and spontaneously attaching the solution using a gravity filtration device, thereby obtaining a hollow fiber ultrafiltration membrane with a base layer introduced into the surface;
[0013] 4. Prepare hydrophilic solution:
[0014] Add manganese chloride and sodium hypochlorite to deionized water, adjust the pH to neutral with concentrated sulfuric acid, stir evenly, and obtain a hydrophilic solution;
[0015] 5. Super-hydrophilic modification of the surface of hollow fiber ultrafiltration membrane:
[0016] The hydrophilic solution is assembled on the surface of the hollow fiber ultrafiltration membrane with the base layer introduced on the surface by means of filtration spontaneous attachment using a gravity filtration device, and further in situ generation is performed on the surface of the hollow fiber ultrafiltration membrane to obtain a modified hollow fiber ultrafiltration membrane;
[0017] 6. The modified hollow fiber ultrafiltration membrane is stored in deionized water to obtain a super hydrophilic hollow fiber membrane.
[0018] Principle of the present invention:
[0019] The present invention firstly utilizes a filtering device to make the nano manganese oxide particles form a loose base layer on the membrane surface, and then utilizes the adsorption of manganese oxide to adsorb the added Mn 2+ Under the catalytic action of manganese oxide, chlorine accelerates the conversion of Mn 2+ The inorganic layer is then converted into manganese oxide, and this step is carried out in the confined space of the base layer, which can generate a more compact coating layer. At this point, the inorganic layer is successfully assembled on the surface of the polymer film.
[0020] The present invention has the following effects:
[0021] 1. The super-hydrophilic modification method of the hollow fiber organic membrane of the present invention is simple, the coating layer thickness is controllable, and the used reagent is green and non-toxic;
[0022] 2. The super hydrophilic hollow fiber organic membrane prepared by the present invention improves the hydrophilicity of the membrane, effectively reduces the adhesion of algae substances, and improves the dynamic anti-fouling property;
[0023] 3. The super hydrophilic layer coated on the hollow fiber organic membrane prepared by the present invention can fall off after being contaminated and then be reassembled, which has high flexibility and prolongs the life of the hollow fiber membrane;
[0024] 4. The polymer hollow fiber membrane filtration and backwashing device prepared by the present invention does not require additional pressurization energy consumption, uses gravity head drive to achieve filtration, and uses filtered water for backwashing, which is low-carbon and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 1 is a physical picture of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0026] Figure 2 The particle size diagram of the manganese oxide colloidal particles prepared in step 2 of Example 1;
[0027] Figure 3 1 is a planar SEM image of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0028] Figure 4 1 is a cross-sectional SEM image of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0029] Figure 5 1 is the element distribution table of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0030] Figure 6 1 is the original membrane and the modified membrane dynamic contact angle diagram, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0031] Figure 7 It is the filtration diagram of the gravity filtration device of the present invention;
[0032] Figure 8 1 is the original hollow fiber ultrafiltration membrane, and 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 2. DETAILED DESCRIPTION
[0033] Specific implementation method 1: This implementation method is a super-hydrophilic modification method of a hollow fiber organic membrane, which is specifically completed by the following steps:
[0034] 1. Pretreatment of organic membrane:
[0035] The hollow fiber ultrafiltration membrane is rinsed with deionized water to obtain a pretreated hollow fiber ultrafiltration membrane;
[0036] 2. Prepare the manganese oxide colloidal particle solution:
[0037] First, add potassium permanganate to deionized water, stir evenly and continuously introduce N 2 Purging was performed to obtain a potassium permanganate solution; then 2 Under the protection of the atmosphere, a sodium thiosulfate solution is dripped into the potassium permanganate solution while stirring; after the dripping is completed, brown manganese oxide colloidal particles are formed, and stirring is continued for a period of time to obtain a manganese oxide colloidal particle solution, which is stored in the dark at 4°C;
[0038] 3. Introducing the base layer on the surface of the hollow fiber ultrafiltration membrane:
[0039] The manganese oxide colloidal particle solution is assembled onto the surface of the pretreated hollow fiber ultrafiltration membrane by filtering and spontaneously attaching the solution using a gravity filtration device, thereby obtaining a hollow fiber ultrafiltration membrane with a base layer introduced into the surface;
[0040] 4. Prepare hydrophilic solution:
[0041] Add manganese chloride and sodium hypochlorite to deionized water, adjust the pH to neutral with concentrated sulfuric acid, stir evenly, and obtain a hydrophilic solution;
[0042] 5. Super-hydrophilic modification of the surface of hollow fiber ultrafiltration membrane:
[0043] The hydrophilic solution is assembled on the surface of the hollow fiber ultrafiltration membrane with the base layer introduced on the surface by means of filtration spontaneous attachment using a gravity filtration device, and further in situ generation is performed on the surface of the hollow fiber ultrafiltration membrane to obtain a modified hollow fiber ultrafiltration membrane;
[0044] 6. The modified hollow fiber ultrafiltration membrane is stored in deionized water to obtain a super hydrophilic hollow fiber membrane.
[0045] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: in step 1, deionized water is used to rinse the hollow fiber ultrafiltration membrane, the pressure difference ΔP between the feed port pressure and the permeate port pressure ranges from 6.0 to 10.0 kPa, and the rinsing time is 15 min to 30 min, thereby obtaining a pretreated hollow fiber ultrafiltration membrane. The other steps are the same as those in specific embodiment 1.
[0046] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the hollow fiber ultrafiltration membrane described in step 1 is a polyethersulfone membrane, a polyvinylidene fluoride membrane, a polyvinylidene fluoride membrane, a cellulose acetate membrane or a polysulfone membrane. The other steps are the same as those of specific embodiment 1 or 2.
[0047] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the concentration of the potassium permanganate solution in step 2 is 0.12 mol / L to 1.2 mol / L; the concentration of the sodium thiosulfate solution in step 2 is 0.06 mol / L to 0.6 mol / L. The other steps are the same as those in specific embodiments 1 to 3.
[0048] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the volume ratio of the potassium permanganate solution and the sodium thiosulfate solution in step 2 is (1 to 1.2): (1 to 1.2). The other steps are the same as those of specific embodiments 1 to 4.
[0049] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the dripping rate in step 2 is 5 mL / min to 10 mL / min, and the stirring speed is 700 r / min to 900 r / min; in step 2, brown manganese oxide colloidal particles are formed, and the stirring time is continued for 12 h to 24 h, and the stirring speed is 700 r / min to 900 r / min. The other steps are the same as those in specific embodiments 1 to 5.
[0050] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 6 in that the filtration time in step 3 is 0 to 30 minutes, and the gravity filtration head is 60 cm to 70 cm. The other steps are the same as those of specific implementation methods 1 to 6.
[0051] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the concentration of manganese chloride in the hydrophilic solution described in step four is 0.5 mg / L to 2 mg / L, and the concentration of sodium hypochlorite is 0.8 mg / L to 3 mg / L; in step four, the pH is adjusted to 6.5 to 7.5 using concentrated sulfuric acid with a concentration of 0.1 mol / L. The other steps are the same as those of specific embodiments one to seven.
[0052] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the time for filtering spontaneous attachment in step 5 is 12 to 24 hours, and the gravity filtering head is 60 to 70 cm. The other steps are the same as those of specific embodiments 1 to 8.
[0053] Specific implementation method ten: This implementation method is a super-hydrophilic modification method of a hollow fiber organic membrane for drinking water purification or wastewater pollution control, and intercepting algae substances in the water.
[0054] The following examples are used to verify the beneficial effects of the present invention:
[0055] Embodiment 1: A method for super-hydrophilic modification of a hollow fiber organic membrane is specifically completed by the following steps:
[0056] 1. Pretreatment of organic membrane:
[0057] The hollow fiber ultrafiltration membrane was rinsed with deionized water, the pressure difference △P between the feed port pressure and the permeate port pressure was in the range of 7.0 kPa, and the rinsing time was 30 minutes, thereby obtaining a pretreated hollow fiber ultrafiltration membrane;
[0058] The hollow fiber ultrafiltration membrane described in step 1 is a polyethersulfone membrane with a molecular cutoff of 100 kD;
[0059] 2. Prepare the manganese oxide colloidal particle solution:
[0060] First, add potassium permanganate to deionized water, stir evenly and continuously introduce N 2 Purging was performed to obtain a potassium permanganate solution; then 2 Under the protection of the atmosphere, sodium thiosulfate solution was dripped into the potassium permanganate solution while stirring; after the dripping was completed, brown manganese oxide colloidal particles were formed, and stirring was continued for 12 hours at a stirring speed of 900 r / min to obtain a manganese oxide colloidal particle solution, which was stored in the dark at 4°C;
[0061] The concentration of the potassium permanganate solution described in step 2 is 0.12 mol / L;
[0062] The concentration of the sodium thiosulfate solution described in step 2 is 0.06 mol / L;
[0063] The volume ratio of the potassium permanganate solution to the sodium thiosulfate solution in step 2 is 1:1;
[0064] The dripping speed in step 2 is 5 mL / min, and the stirring speed is 900 r / min;
[0065] 3. Introducing the base layer on the surface of the hollow fiber ultrafiltration membrane:
[0066] The manganese oxide colloidal particle solution is assembled onto the surface of the pretreated hollow fiber ultrafiltration membrane by filtering and spontaneously attaching the solution using a gravity filtration device, thereby obtaining a hollow fiber ultrafiltration membrane with a base layer introduced into the surface;
[0067] The filtration time in step 3 is 30 min, and the gravity filtration head is 65 cm;
[0068] 4. Prepare hydrophilic solution:
[0069] Add manganese chloride and sodium hypochlorite to deionized water, adjust the pH to 7.0 with 0.1 mol / L concentrated sulfuric acid, stir evenly, and obtain a hydrophilic solution;
[0070] The concentration of manganese chloride in the hydrophilic solution described in step 4 is 0.5 mg / L, and the concentration of sodium hypochlorite is 0.8 mg / L;
[0071] 5. Super-hydrophilic modification of the surface of hollow fiber ultrafiltration membrane:
[0072] The hydrophilic solution is assembled on the surface of the hollow fiber ultrafiltration membrane with the base layer introduced on the surface by means of filtration spontaneous attachment using a gravity filtration device, and further in situ generation is performed on the surface of the hollow fiber ultrafiltration membrane to obtain a modified hollow fiber ultrafiltration membrane;
[0073] The time for filtering spontaneous attachment in step 5 was 0 h, and the gravity filtration head was 65 cm;
[0074] 6. The modified hollow fiber ultrafiltration membrane is stored in deionized water to obtain a super hydrophilic hollow fiber membrane.
[0075] The initial contact angle of the hollow fiber ultrafiltration membrane was 72.0°, and the contact angle was 48.5° after 30s.
[0076] The initial contact angle of the super hydrophilic hollow fiber membrane prepared in Example 1 was 55.8°, and the contact angle was 0.0° after 11 seconds.
[0077] Example 2: The difference between this example and Example 1 is that the filtration time in step 3 is 10 minutes, and the filtration time for spontaneous attachment in step 5 is 12 hours. The other steps and parameters are the same as those in Example 1.
[0078] The initial contact angle of the super hydrophilic hollow fiber membrane prepared in Example 2 was 0.0°.
[0079] Figure 1 1 is a physical picture of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0080] from Figure 1 It can be seen from the appearance that the nano-manganese oxide armor was successfully assembled on the hollow fiber membrane. The surface of the membrane with only the assembled base layer appeared brown, and after further coating with a super hydrophilic layer, the color of the membrane continued to deepen, showing a significant metallic luster.
[0081] Figure 2 The particle size diagram of the manganese oxide colloidal particles prepared in step 2 of Example 1;
[0082] Figure 2It shows that the prepared manganese oxide particles are nanoparticles.
[0083] Figure 3 1 is a planar SEM image of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0084] Depend on Figure 3 It can be seen that the original surface of the hollow fiber ultrafiltration membrane has uniform pore size. After filtering the manganese oxide particle base layer under gravity, the pores on the membrane surface are covered, and then a fold-like coating layer is formed. After the super hydrophilic layer continues to grow and assemble on the base layer, neatly arranged manganese oxide clusters appear above the folds on the membrane surface, and the thickness of the modified layer increases.
[0085] Figure 4 1 is a cross-sectional SEM image of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0086] Depend on Figure 4 It can be seen that the assembly of the base layer causes a relatively flat shell-like surface to appear on the outer surface of the hollow ultrafiltration membrane. Then, with the assembly of the superhydrophilic layer, evenly arranged spherical blankets continue to grow on the shell-like surface, increasing the specific surface area of the membrane surface.
[0087] Figure 5 1 is the element distribution table of the original membrane and the modified membrane, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0088] Depend on Figure 5 It can be seen that there is no Mn element on the original surface of the hollow ultrafiltration membrane. With the coating of the base layer and the super hydrophilic layer, the Mn element on the membrane surface increases gradually. Combined with the SEM image, the successful assembly of the manganese oxide armor is further confirmed.
[0089] In order to measure the change of water contact angle on the membrane surface before and after manganese oxide coating modification, the contact angle of the membrane surface was measured by a contact angle meter (JYSP180 contact angle meter, Jinxinsheng, Beijing). The hollow fiber membrane was dried at room temperature before the test. After the membrane was dried, it was smoothly glued to the glass slide with double-sided tape to ensure that it was horizontal for measurement. The contact angle was measured by the fixed drop method: the prepared membrane sample was placed on a horizontal stage, and the image shooting and recording software equipped with the instrument was turned on to record the image of the droplet to be measured fixed on the membrane surface; 2μL of the droplet to be measured was transferred to the membrane surface with a 10μL pipette, and the morphological changes of the droplet fixed on the membrane surface within 30s were continuously recorded and the image was saved. In order to reduce the influence of accidental experimental errors, the hollow fiber membrane under the same modification conditions was measured at least 3 times, and the average value of multiple measurements was finally taken as the water contact angle of the modified membrane.
[0090] Figure 6 1 is the original membrane and the modified membrane dynamic contact angle diagram, in which 1 is the original hollow fiber ultrafiltration membrane, 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 1, and 3 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0091] Depend on Figure 6 It can be seen that the original hollow fiber membrane is a hydrophilic membrane, and the water contact angle is stable at about 48.5°. After assembling the base layer, the hydrophilicity is improved to a certain extent, and its initial water contact angle is 55.8°, which can drop to 0.0° after 11s. After in-situ modification of the super hydrophilic layer, the hydrophilicity is greatly improved, and its initial water contact angle is 0.0°. The reason for this phenomenon is that manganese oxide is a hydrophilic substance. After in-situ generation, under the catalysis of the manganese oxide particles in the base layer, the solution of manganese chloride will be accelerated to oxidize, and manganese oxide particles will be formed in the nano-confinement between the pores of the base layer. Therefore, the coated manganese oxide layer is denser and the hydrophilicity is further improved.
[0092] Figure 7 It is the filtration diagram of the gravity filtration device of the present invention; Figure 7 For existing devices, use deionized water to prepare 1*10 5 cell / mL of Microcystis aeruginosa algae liquid was used as the contaminated liquid, and the filtration performance was tested using a gravity pressure filtration device;
[0093] Figure 7 ① in the middle is a valve: controls opening and closing;
[0094] ② Valve: control opening and closing, connect to the atmosphere, and remove bubbles in the device;
[0095] ③ Valve: controls opening and closing, used for draining water;
[0096] ④ Pressure gauge: for testing the internal water pressure of the device;
[0097] When the device is running, valves ① and ② are opened, ③ is closed, and the water tank is filled with Microcystis aeruginosa liquid and then enters the membrane assembly. After the bubbles in the device are emptied, valve ② is closed and the membrane water flux test is started. A balance is placed under the outlet for measurement to obtain the membrane water flux data. After the device is finished running, valve ① is closed and valve ③ is opened to drain water. If filtration modification is performed, the solution in the sewage tank can be replaced with the modified solution.
[0098] Figure 8 1 is the original membrane and the modified membrane dynamic filtration flux change curve, in which 1 is the original hollow fiber ultrafiltration membrane, and 2 is the super hydrophilic hollow fiber organic membrane prepared in Example 2;
[0099] Depend on Figure 8 It can be seen that the specific flux of the original ultrafiltration membrane in treating algae-containing water drops rapidly in the initial stage of filtration, while the decline trend of the modified membrane is alleviated. This is because in the initial stage of filtration, algae cells quickly settle to the surface of the ultrafiltration membrane and quickly form a filter cake layer. The hydrophilicity of the modified membrane is enhanced, which weakens the adhesion of algae cells.
Claims
1. A method for super-hydrophilic modification of hollow fiber organic membrane, characterized in that The method is specifically completed according to the following steps:
1. Pretreatment of organic membrane: The hollow fiber ultrafiltration membrane is rinsed with deionized water to obtain a pretreated hollow fiber ultrafiltration membrane; 2. Prepare the manganese oxide colloidal particle solution: First, potassium permanganate is added to deionized water, stirred evenly and N2 is continuously introduced for purging to obtain a potassium permanganate solution; then, sodium thiosulfate solution is dripped into the potassium permanganate solution under the protection of N2 atmosphere, and stirring is performed while dripping; after the dripping is completed, brown manganese oxide colloidal particles are formed, and stirring is continued for a period of time to obtain a manganese oxide colloidal particle solution, which is stored in the dark at 4°C; 3. Introducing the base layer on the surface of the hollow fiber ultrafiltration membrane: The manganese oxide colloidal particle solution is assembled onto the surface of the pretreated hollow fiber ultrafiltration membrane by filtering and spontaneously attaching the solution using a gravity filtration device, thereby obtaining a hollow fiber ultrafiltration membrane with a base layer introduced into the surface; 4. Prepare hydrophilic solution: Add manganese chloride and sodium hypochlorite to deionized water, adjust the pH to neutral with concentrated sulfuric acid, stir evenly, and obtain a hydrophilic solution; 5. Super-hydrophilic modification of the surface of hollow fiber ultrafiltration membrane: The hydrophilic solution is assembled on the surface of the hollow fiber ultrafiltration membrane with the base layer introduced on the surface by means of filtration spontaneous attachment using a gravity filtration device, and further in situ generation is performed on the surface of the hollow fiber ultrafiltration membrane to obtain a modified hollow fiber ultrafiltration membrane; 6. The modified hollow fiber ultrafiltration membrane is stored in deionized water to obtain a super hydrophilic hollow fiber membrane.
2. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that In step 1, the hollow fiber ultrafiltration membrane is rinsed with deionized water, the pressure difference ΔP between the feed port pressure and the permeate port pressure ranges from 6.0 to 10.0 kPa, and the rinsing time is 15 min to 30 min, thereby obtaining a pretreated hollow fiber ultrafiltration membrane.
3. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The hollow fiber ultrafiltration membrane described in step 1 is a polyethersulfone membrane, a polyvinylidene fluoride membrane, a polyvinylidene fluoride membrane, a cellulose acetate membrane or a polysulfone membrane.
4. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The concentration of the potassium permanganate solution in step 2 is 0.12 mol / L to 1.2 mol / L; the concentration of the sodium thiosulfate solution in step 2 is 0.06 mol / L to 0.6 mol / L.
5. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The volume ratio of the potassium permanganate solution and the sodium thiosulfate solution described in step 2 is (1-1.2):(1-1.2).
6. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The dripping rate in step 2 is 5 mL / min to 10 mL / min, and the stirring speed is 700 r / min to 900 r / min. In step 2, brown manganese oxide colloidal particles are formed, and the stirring time is continued for 12 h to 24 h, and the stirring speed is 700 r / min to 900 r / min.
7. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The filtration time in step three is 0 to 30 minutes, and the gravity filtration head is 60 cm to 70 cm.
8. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The concentration of manganese chloride in the hydrophilic solution in step 4 is 0.5 mg / L to 2 mg / L, and the concentration of sodium hypochlorite is 0.8 mg / L to 3 mg / L; in step 4, the pH is adjusted to 6.5 to 7.5 using concentrated sulfuric acid with a concentration of 0.1 mol / L.
9. The method for super-hydrophilic modification of a hollow fiber organic membrane according to claim 1, characterized in that The time for spontaneous attachment by filtration in step 5 is 12 to 24 hours, and the water head for gravity filtration is 60 to 70 cm.
10. Application of the super-hydrophilic modification method of a hollow fiber organic membrane prepared by the preparation method according to claim 1, characterized in that A super-hydrophilic modification method of a hollow fiber organic membrane is used for drinking water purification or wastewater pollution control to intercept algae substances in the water.
Citation Information
Patent Citations
Method for preparing layered humic acid / manganese oxide composite catalyst from humic acid and application of layered humic acid / manganese oxide composite catalyst
CN115430461A
Modification method for in-situ growth of manganese dioxide on surface of ultrafiltration membrane based on metal polyphenol network
CN115463564A
Flower arrangement
KR102165961B1
Filter Membrane Modifying Method Based On Metallic Oxide Particles
US20210197131A1