Zirconium phosphate-based composite material as well as preparation method and application thereof
The zirconium phosphate-based composite material prepared by hydrothermal crystallization solves the problem of poor ammonium removal effect in cell culture medium in the prior art, realizes efficient ammonium removal and medium recycling, and supports the ability of bioreactors Continuous development.
Patent Information
- Application Number
- CN202310522699.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing zirconium phosphate and its derivatives are poor in removing ammonium in cell culture media, affecting cell growth and recycling of culture media, resulting in high cost and sustainable development challenges.
By mixing soluble zirconium source, hydrated phosphate and mineralizer, zirconium phosphate-based composite material with a two-dimensional sheet structure is prepared by hydrothermal crystallization, and the removal of ammonium is improved by using its broad ionic channels and high hydrophilicity. Efficiency and multiple cycles.
This method significantly improves the ammonium removal effect in the water system and cell culture medium, ensures normal cell growth, and reduces the frequency and cost of medium replacement, supporting the sustainable operation of the bioreactor.
Smart Images

Figure CN118925653A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorbents, and specifically relates to a zirconium phosphate-based composite material and a preparation method and application thereof. Background Art
[0002] During high-density cell culture, cells will quickly consume nutrients such as glucose and glutamine, and produce metabolic byproducts such as ammonia, lactic acid and carbonic acid. Among them, ammonium is considered to be a toxic substance that inhibits cell growth. The accumulation of ammonia will affect cell growth and the production of recombinant proteins, change the electrochemical gradient of the cell compartment, impair the enzyme activity in the cell body, and induce cell apoptosis. When the concentration of ammonia accumulates to a certain level, the cell culture medium must be replaced in time to maintain the normal life activities of the cells. The cost of cell culture medium is high, especially fetal bovine serum, growth factors and nutrients. Therefore, for the future operation of large-scale bioreactors, it is necessary to minimize the inhibitory effect of metabolic byproducts on cells, achieve efficient recycling of culture medium as much as possible, and ensure the sustainable development of cell agriculture.
[0003] Layered materials are a new type of material, especially zirconium phosphate and its derivatives, which have many applications such as flame retardancy, ion exchange, catalysis, and antibacterial. Research on zirconium phosphate and its derivatives in removing heavy metals from sewage, fixing radioactive elements and rare earth elements from nuclear pollution is becoming increasingly abundant. Some preliminary studies have confirmed that zirconium phosphate can adsorb ammonia and can achieve multiple cycles; at the same time, in the field of medical kidney dialysis, it can be used as an ion exchanger for cations.
[0004] Due to the complex composition and numerous competing cations in cell culture medium, existing zirconium phosphate and its derivatives are not effective in removing ammonium from the culture medium. Summary of the invention
[0005] The object of the present invention is to provide a zirconium phosphate-based composite material and a preparation method and application thereof. The zirconium phosphate-based composite material prepared by the method provided by the present invention has a high removal effect on ammonium in a water system or a cell culture medium.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a zirconium phosphate-based composite material, comprising the following steps:
[0008] A soluble zirconium source, a hydrated phosphate and a mineralizer are mixed and subjected to hydrothermal crystallization to obtain the zirconium phosphate-based composite material;
[0009] The number of crystal water in the hydrated phosphate is ≥2.
[0010] Preferably, the soluble zirconium source includes one or more of zirconium oxychloride octahydrate, zirconium nitrate and zirconium sulfate.
[0011] Preferably, the hydrated phosphate includes one or more of dihydrogen phosphate, hydrogen phosphate, metaphosphate and orthophosphate;
[0012] The cations in the hydrated phosphate include sodium ions, potassium ions, calcium ions or magnesium ions.
[0013] Preferably, the mineralizer includes one or more of sodium fluoride, hydrofluoric acid and ammonium fluoride.
[0014] Preferably, the molar ratio of the soluble zirconium source to the hydrated phosphate is 1:1-5, calculated on the basis of the molar amounts of Zr and P, respectively.
[0015] Preferably, the molar ratio of the hydrated phosphate to the mineralizer is 5 to 15:1.
[0016] Preferably, the temperature of the hydrothermal crystallization is 100-120° C., and the insulation time is 12-36 hours.
[0017] The present invention also provides a zirconium phosphate-based composite material prepared by the preparation method described in the above technical solution, wherein the zirconium phosphate-based composite material has a two-dimensional lamellar structure;
[0018] The particle size of the zirconium phosphate-based composite material is 300 to 1400 nm; the interlayer spacing of the two-dimensional sheet structure is
[0019] The crystallinity of the zirconium phosphate-based composite material is 68-75%.
[0020] The present invention also provides the use of the zirconium phosphate-based composite material described in the above technical solution in the adsorption of ammonium.
[0021] Preferably, the ammonium includes ammonium in aqueous solution or ammonium in cell culture medium.
[0022] The present invention provides a method for preparing a zirconium phosphate-based composite material, comprising the following steps: mixing a soluble zirconium source, a hydrated phosphate and a mineralizer, and subjecting the mixture to hydrothermal crystallization to obtain the zirconium phosphate-based composite material; the number of crystal waters in the hydrated phosphate is ≥2. In the present invention, a hydrated phosphate containing more than 2 crystal waters is used as a raw material, which can improve the crystallinity of the crystals, form a wider and more regular ion channel, and improve the ion adsorption capacity; at the same time, the crystal water in the raw material can increase the hydrophilicity of the crystals, accelerate the ion exchange rate, and thus make the obtained composite material have a higher removal efficiency for ammonium in the water system or cell culture medium; and the obtained composite material has good biocompatibility, has little effect on the pH of the system, and can be recycled for many times. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the sodium zirconium phosphate obtained in Example 1;
[0024] Figure 2 This is a SEM image of the sodium zirconium phosphate obtained in Comparative Example 1;
[0025] Figure 3 The particle size distribution diagram of sodium zirconium phosphate obtained in Example 1 and Comparative Example 1;
[0026] Figure 4 The contact angle test diagram of sodium zirconium phosphate obtained in Example 1 and Comparative Example 1;
[0027] Figure 5 The figure is a biological toxicity test result diagram of sodium zirconium phosphate obtained in Example 1 and Comparative Example 1;
[0028] Figure 6 This is a diagram showing the effect of sodium zirconium phosphate obtained in Example 1 on the removal of ammonium in cell culture medium;
[0029] Figure 7 This is a physical picture of the mixed liquid obtained after manual grinding in Example 1;
[0030] Figure 8 This is a physical picture of the mixed liquid obtained after manual grinding in Comparative Example 1;
[0031] Fig. 9 This is a diagram showing the removal effect of the sodium zirconium phosphate obtained in Example 1 when it is reused in an aqueous solution. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing a zirconium phosphate-based composite material, comprising the following steps:
[0033] A soluble zirconium source, a hydrated phosphate and a mineralizer are mixed and subjected to hydrothermal crystallization to obtain the zirconium phosphate-based composite material;
[0034] The number of crystal water in the hydrated phosphate is ≥2.
[0035] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0036] In the present invention, the number of the crystal water is ≥2, more preferably 2, 7 or 12.
[0037] In the present invention, the soluble zirconium source preferably includes one or more of zirconium oxychloride octahydrate, zirconium nitrate and zirconium sulfate.
[0038] In the present invention, the hydrated phosphate preferably includes one or more of dihydrogen phosphate, hydrogen phosphate, metaphosphate and orthophosphate. In the present invention, the cation in the hydrated phosphate preferably includes sodium ion, potassium ion, calcium ion or magnesium ion. In a specific embodiment of the present invention, the hydrated phosphate is specifically disodium hydrogen phosphate dodecahydrate.
[0039] In the present invention, the molar ratio of the soluble zirconium source to the hydrated phosphate is preferably 1:1-5, more preferably 1:2-4, and even more preferably 1:3, calculated on the molar basis of Zr and P, respectively.
[0040] In the present invention, the mineralizer preferably includes one or more of sodium fluoride, hydrofluoric acid and ammonium fluoride. In the present invention, the molar ratio of the hydrated phosphate to the mineralizer is preferably 5 to 15:1, more preferably 8 to 12:1, and more preferably 10 to 11:1. In the present invention, the mineralizer can increase the stability of the crystal.
[0041] The present invention has no special limitation on the mixing process, and a method known to those skilled in the art can be used. In a specific embodiment of the present invention, the mixing method is preferably manual grinding; the manual grinding time is preferably 10 to 20 minutes. The present invention can release the crystal water in the raw material by grinding, which serves as a solvent liquid in the hydrothermal crystallization process to make the crystal uniform.
[0042] In the present invention, the temperature of the hydrothermal crystallization is preferably 100-120° C., more preferably 105-110° C.; the insulation time is preferably 12-36 h, more preferably 18-30 h, and more preferably 24 h.
[0043] In the present invention, the hydrothermal crystallization process preferably includes:
[0044] The mixed material obtained by mixing is placed in a polypropylene reaction bottle, the bottle cap is tightly closed, and then the polypropylene reaction bottle is placed in an oven for heating to perform hydrothermal crystallization.
[0045] After the hydrothermal crystallization, the present invention also preferably includes sequentially washing, filtering, drying and grinding the obtained reaction liquid.
[0046] The present invention has no particular limitation on the washing and filtering process, and those familiar to those skilled in the art may be used.
[0047] In the present invention, the drying method is preferably: drying in an oven at 60° C. overnight.
[0048] The present invention has no particular limitation on the grinding process, and any method known to those skilled in the art may be used.
[0049] The preparation method provided by the invention is simple and can realize scaled-up production.
[0050] The present invention also provides a zirconium phosphate-based composite material prepared by the preparation method described in the above technical solution. In the present invention, the zirconium phosphate-based composite material preferably includes sodium zirconium phosphate. In the present invention, the zirconium phosphate-based composite material has a two-dimensional lamellar structure. In the present invention, the particle size of the zirconium phosphate-based composite material is preferably 300 to 1400 nm, more preferably 500 to 1200 nm, and more preferably 800 to 1000 nm. In the present invention, the interlayer spacing of the two-dimensional lamellar structure is preferably More preferably In the present invention, the crystallinity of the zirconium phosphate-based composite material is preferably 68-75%, and more preferably 73.7%.
[0051] The present invention also provides the use of the zirconium phosphate-based composite material described in the above technical solution in the adsorption of ammonium.
[0052] In the present invention, the ammonium preferably includes ammonium in an aqueous solution or ammonium in a cell culture medium.
[0053] In the present invention, when the zirconium phosphate-based composite material is used to adsorb ammonium in an aqueous solution, the adsorption process preferably includes:
[0054] The zirconium phosphate-based composite material and the aqueous solution containing ammonium are mixed, the obtained mixed liquid is placed in a conical flask, and the conical flask is placed in a constant temperature shaker for shaking.
[0055] In the present invention, the concentration of ammonium in the aqueous solution containing ammonium is preferably 0.1 to 20 mmol / L. In the present invention, the pH value of the aqueous solution containing ammonium is preferably 6.5 to 7.5, and more preferably 6.8 to 7.3. In the present invention, the dosage ratio of the zirconium phosphate-based composite material to the aqueous solution containing ammonium is preferably 2.5 to 20 g: 1 L.
[0056] In the present invention, the temperature of the thermostatic shaker is preferably 37° C. In the present invention, the rotation speed of the thermostatic shaker is preferably 150 rpm, and the oscillation time is preferably 30 min.
[0057] After the oscillation, the present invention further preferably includes detecting the mixed system after the oscillation, and the detection process preferably includes:
[0058] The sample was taken with a disposable syringe, filtered through a filter membrane with a pore size of 0.22 μm, and the filtrate was collected to detect the changes in ammonium concentration and pH value in the filtrate.
[0059] The present invention has no particular limitation on the specific detection method for the change in ammonium concentration and pH value, and any method known to those skilled in the art may be used.
[0060] In the present invention, when the zirconium phosphate-based composite material is used to adsorb ammonium in a cell culture medium, the adsorption process preferably includes:
[0061] The zirconium phosphate-based composite material and the cell culture medium containing ammonium are mixed, the obtained mixed liquid is placed in a conical flask, and the conical flask is placed in a constant temperature shaker for shaking.
[0062] The present invention has no particular limitation on the source of the cell culture medium containing ammonium, and any type of cell culture medium containing ammonium may be used.
[0063] In the present invention, the concentration of ammonium in the ammonium-containing cell culture medium is preferably 0.1 to 20 mmol / L. In the present invention, the pH value of the ammonium-containing cell culture medium is preferably 7.0 to 7.4, and more preferably 7.2 to 7.4. In the present invention, the dosage ratio of the zirconium phosphate-based composite material to the ammonium-containing cell culture medium is preferably 2.5 to 20 g: 1 L.
[0064] In the present invention, the temperature of the thermostatic shaker is preferably 37° C. In the present invention, the rotation speed of the thermostatic shaker is preferably 150 rpm, and the oscillation time is preferably 30 min.
[0065] After the oscillation, the present invention further preferably includes detecting the mixed system after the oscillation, and the detection process preferably includes:
[0066] The sample was taken with a disposable syringe, filtered through a 0.22 μm filter membrane, and the filtrate was collected to detect the changes in ammonium concentration and pH value in the filtrate.
[0067] The present invention has no particular limitation on the specific detection method for the change in ammonium concentration and pH value, and any method known to those skilled in the art may be used.
[0068] The zirconium phosphate-based composite material provided by the present invention is used as an adsorbent for ammonium in a cell culture medium, which can be used to reduce the toxic effects caused by ammonium accumulation during animal cell culture and is conducive to the recycling of cell culture medium during high-density cell culture.
[0069] In order to further illustrate the present invention, a zirconium phosphate-based composite material provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0070] Example 1
[0071] 3.222g zirconium oxychloride octahydrate, 10.744g disodium hydrogen phosphate dodecahydrate and 0.126g sodium fluoride were mixed and put into a mortar for manual grinding for 15 minutes. Figure 7 The reaction mixture was transferred into a 30 mL brown polypropylene reaction bottle, the bottle cap was tightly closed, and the reaction mixture was placed in an oven at 105° C. for hydrothermal crystallization and kept warm for 24 h. The obtained reaction liquid was washed with water, filtered, dried overnight at 60° C., and then ground to obtain sodium zirconium phosphate (labeled as α-Na2ZrPA, with a crystallinity of 73.7% and an interlayer spacing of ).
[0072] Comparative Example 1
[0073] 3.222 g of zirconium oxychloride octahydrate, 4.258 g of anhydrous disodium hydrogen phosphate and 0.126 g of sodium fluoride were mixed and put into a mortar for manual grinding for 15 min. Figure 8 The mixture was transferred to a 30 mL brown polypropylene reaction bottle, the bottle cap was tightly closed, and the reaction solution was placed in an oven at 105° C. for thermal crystallization and kept warm for 24 h. The obtained reaction solution was washed with water, filtered, dried at 60° C. overnight, and then ground to obtain sodium zirconium phosphate with a particle size of 300 nm (labeled as α-Na2ZrP B, with a crystallinity of 65.1% and an interlayer spacing of ).
[0074] Application Example 1
[0075] Weigh 50 mg of the sodium zirconium phosphate obtained in Example 1 and Comparative Example 1 respectively, add them into a conical flask containing 20 mL of 50 mmol / L NH4Cl aqueous solution with a pH of 7.3, cover with a rubber stopper, put in a constant temperature shaker at a temperature of 37°C and a speed of 150 rpm, and shake for 30 minutes;
[0076] After the end, a disposable syringe was used to take a sample, and after filtering through a filter membrane with a pore size of 0.22 μm, the filtrate was collected to detect the changes in the ammonium concentration and the pH of the solution;
[0077] The test results showed that the adsorption capacity of α-Na2ZrP A and α-Na2ZrP B for ammonium were 5.61±0.09mmol / g and 5.33±0.45mmol / g, respectively, and the pH of the solutions increased by 0.58±0.01 and 0.65±0.02, respectively.
[0078] Application Example 2
[0079] 26.87 mg NH4Cl was dissolved in 100 mL DMEM high glucose medium without phenol red and sodium pyruvate (Wuhan Punosai Life Science Technology Co., Ltd., China) to prepare NH4+ The culture medium with a concentration of 50 mM was diluted tenfold to serve as the test solution;
[0080] Weigh 50 mg, 100 mg, and 200 mg of the adsorbent obtained in Example 1 respectively and put them into 30 mL glass sample bottles, then add 10 mL of the test solution, cover the bottles tightly, and place them in a shaker at 37° C. and 150 rpm for 30 min;
[0081] After the end, a disposable syringe was used to take a sample, and after filtering through an organic filter membrane with a pore size of 0.22 μm, the filtrate was collected and tested for NH4 + The pH value of the culture medium was determined by using a pH meter (Ray PHSJ-4F, Shanghai Yidian Scientific Instrument Co., Ltd., China); the urea nitrogen kit (Cat. No. C013-2, Nanjing Jiancheng Biological Co., Ltd., China) was used to determine the NH4 + The concentration of NH4 before and after adsorption was determined by making a standard curve. + concentration;
[0082] Test results such as Figure 6 As shown, from Figure 6 It can be seen that the sodium zirconium phosphate α-Na2ZrPA obtained in Example 1 has a high activity against 5mM NH4 at three dosages of 5g / L, 10g / L and 20g / L. + The removal efficiencies of Na and NH were 19.88%, 28.25% and 38.09% respectively. The pH of the culture medium system only fluctuated slightly, because with the increase of the dosage, Na + With NH4 + The exchange capacity increases, and the NH4 + It is gradually transferred to the adsorbent, so the pH of the solution increases slightly;
[0083] In addition, the precipitation amount of the adsorbent during the adsorption process was tested. + The precipitation amount of Zr4 increases with the increase of adsorbent dosage, but at a dosage of 20 g / L, + The precipitation amount is only 4.23 mg / L.
[0084] Application Example 3
[0085] In order to increase the ammonium concentration in the culture medium, a complete culture medium that had been placed in a refrigerator at 4°C for a period of time was selected, which was DMEM (gibco, ThermoFisher Biochemical Products (Beijing) Co., Ltd.) culture medium containing 10% fetal bovine serum;
[0086] Mouse myoblasts (C2C12) were seeded in 90×15 mm cell culture dishes at a seeding density of 9.25×104 cells / mL, add 10mL complete medium, and culture in an incubator at 37°C, 5% CO2, and 95% humidity for three days; the concentration of ammonium in the test cell culture medium is 15.99mM;
[0087] 80 mg of the sodium zirconium phosphate α-Na2ZrPA adsorbent prepared in Example 1 was added to a 20 mL glass bottle, and 4 mL of cell culture fluid after culturing cells was added, and the mixture was shaken in a shaker at 37°C and 150 rpm for 30 minutes; the test results showed that after the adsorbent was added, the ammonium concentration in the culture medium decreased by 25.94±8.39%.
[0088] Performance Testing
[0089] Test Example 1
[0090] The sodium zirconium phosphate obtained in Example 1 and Comparative Example 1 was subjected to scanning electron microscopy test and flake size distribution test, and the obtained SEM images are as follows: Figures 1-2 As shown, Figure 1 For Example 1, Figure 2 For Example 2, the sheet diameter distribution diagram is as follows Figure 3 As shown, from Figures 1 to 3 It can be seen that the two adsorbents are dispersed relatively evenly and present a flake structure;
[0091] The nanoparticle size of α-Na2ZrPA is relatively large, about 1.4μm, while the particle size of α-Na2ZrPB is smaller, with an average particle size of about 300nm; this is related to the surface water content during the material synthesis process. There is more surface bound water in α-Na2ZrPA. When the tiny crystals grow to a certain scale, the crystals aggregate under the connection of hydrogen bonds in water molecules to form crystal adhesion, and the grain size increases, resulting in its average particle size being much larger than α-Na2ZrPB.
[0092] Test Example 2
[0093] The hydrophilicity and hydrophobicity of the sodium zirconium phosphate obtained in Example 1 and Comparative Example 1 were tested, and the contact angles obtained were as follows: Figure 4 As shown, from Figure 4 It can be seen that the contact angle of α-Na2ZrPA is smaller than that of α-Na2ZrPB, indicating that α-Na2ZrPA is more hydrophilic than α-Na2ZrPB.
[0094] Test Example 3
[0095] Testing the biocompatibility of the sodium zirconium phosphate obtained in Example 1:
[0096] Refer to GB / T 16886.5-2017 "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Test" for cytotoxicity test of adsorbents;
[0097] Weigh 5-25 mg of the adsorbent prepared in Example 1 and put it into a glass bottle for wet heat sterilization, add 10 mL of culture medium containing 10% fetal bovine serum, and place it in a refrigerator at 4°C for 24±2 hours. After sterile filtration, inoculate cells;
[0098] 50 μL of C2C12 cells that have been passaged for 2 to 3 generations were inoculated into a 24-well plate, with the inoculation number being about 1×10 per well. 5 450 μL of the soaked culture medium was added and the cells were cultured in an incubator containing 5% CO2. After 24 hours of culture, the cell morphology was observed under a microscope, and then 10% volume of Cell Counting kit-8 (CCK8) reagent was added and incubated for 1 hour. 100 μL of liquid was added to each well of the 96-well plate, and the CCK-8 reagent solution was used as the blank group. The OD value was measured at a wavelength of 450 nm using an enzyme marker to indirectly reflect the number of living cells.
[0099] Each set of experiments was repeated three times, and two OD values were measured each time. After the test, 500 μL of the corresponding culture medium was added to each well and continued to incubate. The relative cell survival rate was calculated to determine the cell survival status; the test results are shown in Figure 5 shown; from Figure 5 The results show that after 24 hours of culture, the cell survival rate of all immersion concentration experimental groups is above 80%, and the microscopic morphology is no different from that of the blank control group, and the cells are in a healthy state. This shows that the zirconium phosphate-based composite material provided by the present invention has good biocompatibility and potential for application in the fields of biomedicine and cell food.
[0100] Test Example 4
[0101] The reusability of the sodium zirconium phosphate obtained in Example 1 for adsorbing 5 mM ammonium in aqueous solution was measured. The adsorbent was rinsed with distilled water, dried at 60-80°C, and then used again. Fig. 9 It can be seen that after repeated use three times, sodium zirconium phosphate maintains a similar adsorption effect.
[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a zirconium phosphate-based composite material, characterized in that: The following steps are involved: A soluble zirconium source, a hydrated phosphate and a mineralizer are mixed and subjected to hydrothermal crystallization to obtain the zirconium phosphate-based composite material; The number of crystal water in the hydrated phosphate is ≥2.
2. The preparation method according to claim 1, characterized in that: The soluble zirconium source includes one or more of zirconium oxychloride octahydrate, zirconium nitrate and zirconium sulfate.
3. The preparation method according to claim 1, characterized in that: The hydrated phosphate includes one or more of dihydrogen phosphate, hydrogen phosphate, metaphosphate and orthophosphate; The cations in the hydrated phosphate include sodium ions, potassium ions, calcium ions or magnesium ions.
4. The preparation method according to claim 1, characterized in that: The mineralizer includes one or more of sodium fluoride, hydrofluoric acid and ammonium fluoride.
5. The preparation method according to claim 1, characterized in that: Calculated by the molar amounts of Zr and P respectively, the molar ratio of the soluble zirconium source to the hydrated phosphate is 1:1-5.
6. The preparation method according to claim 5, characterized in that: The molar ratio of the hydrated phosphate to the mineralizer is 5-15:
1.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The temperature of the hydrothermal crystallization is 100-120° C., and the insulation time is 12-36 hours.
8. The zirconium phosphate-based composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The zirconium phosphate-based composite material has a two-dimensional lamellar structure; The particle size of the zirconium phosphate-based composite material is 300 to 1400 nm; the interlayer spacing of the two-dimensional sheet structure is The crystallinity of the zirconium phosphate-based composite material is 68-75%.
9. Use of the zirconium phosphate-based composite material according to claim 8 in adsorbing ammonium.
10. The use according to claim 9, characterized in that: The ammonium includes ammonium in aqueous solution or ammonium in cell culture medium.
Citation Information
Patent Citations
Preparation method of nanoflower zirconium phosphate adsorbent
CN106902784A
Micron-scale lamellar zirconium phosphate and preparation method thereof
CN108910854A
Production of crystalline zirconium phosphate compound
JP1993017112A
Zirconium phosphate particles, and method for manufacturing the same
JP2016037408A