SiO2 aerogel as well as preparation method and application thereof

By modifying the composite amine on the SiO2 aerogel, a SiO2 aerogel with high pore volume and high specific surface area is formed, which solves the problems of small adsorption capacity and poor selectivity of the existing CO2 absorber, and achieves high-efficiency and low-energy consumption CO2 capture and regeneration reduces costs and energy consumption.

CN118925674APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310757600.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2023-06-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing CO2 absorber has small operating adsorption capacity and poor selectivity, especially when used under low pressure, the above defects are more obvious, and the liquid amine absorption-regeneration technology has problems such as high cost, complex equipment, and large energy consumption.

Method used

SiO2 aerogel is used as an adsorbent to improve its pore volume, specific surface area and porosity through composite amine modification. The preparation method includes impregnation, ultrasonication and nitrogen purge to form SiO2 with low density, large specific surface area and high porosity. Aerogel, used for CO2 capture and regeneration.

Benefits of technology

It achieves high-efficiency, low-energy consumption and low-cost CO2 adsorption and regeneration performance, and can be recycled multiple times, reducing regeneration energy consumption, and improving the efficiency and modularity of the CO2 absorption module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004303405560000111
    Figure BDA0004303405560000111
  • Figure BDA0004303405560000121
    Figure BDA0004303405560000121
  • Figure BDA0004303405560000122
    Figure BDA0004303405560000122
Patent Text Reader

Abstract

The invention relates to the technical field of gas separation, and discloses SiO2 aerogel as well as a preparation method and application thereof. The SiO2 aerogel is SiO2 aerogel loaded by composite amine, and the molecular weight of the SiO2 aerogel is 100-200. The pore volume is 0.8-1.5 cm < 3 > / g, the specific surface area is 200-850 m < 2 > / g, and the porosity is 75-99.5%; the volume fraction of the SiO2 skeleton is less than 10%, and the volume fraction of the three-dimensional grid void is greater than or equal to 90%. The SiO2 aerogel has the characteristics of low density, large specific surface area, high porosity and excellent adsorption and regeneration performance, and the preparation method is low in cost and convenient in technological process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of gas separation, and in particular to a SiO2 aerogel and a preparation method and application thereof. Background Art

[0002] Greenhouse gases, mainly CO2, emitted from the combustion of fossil energy have become the main factor affecting global climate change. Many countries and scientists are facing tremendous pressure to reduce CO2 emissions and the challenge of developing effective CO2 capture and utilization systems. At the same time, carbon dioxide is also a potential carbon resource. Recycling and utilizing carbon dioxide is conducive to the recycling of carbon resources. Therefore, many countries are committed to the research on carbon dioxide separation, capture and utilization. It is quite difficult for the CO2 capture, separation and recovery system to achieve stable operation and low cost under complex flue gas conditions. This is also the fundamental reason why it is difficult to make breakthrough progress in flue gas CO2 capture and recovery technology.

[0003] At present, the capture and separation technologies of carbon dioxide in flue gas include liquid solvent absorption, adsorption, biological method, membrane separation and low-temperature freezing, etc. Among them, the liquid solvent absorption-regeneration process is relatively mature and has been applied in the petrochemical industry. Commonly used absorbents include liquid amine absorbents such as monoethanolamine, diethanolamine, and N-methyldiethanolamine solution. Liquid amine absorbents have the advantages of fast absorption speed, strong absorption capacity, and easy regeneration. However, liquid amine absorption-regeneration technology still has defects such as high cost, easy corrosion of equipment pipelines, high energy consumption of absorbent regeneration, and easy degradation of absorbents. The existing CO2 absorbent has low working adsorption capacity and poor adsorption selectivity, especially when used at lower pressures. The above defects are more obvious. When the processing volume increases, the number of adsorption beds increases, which correspondingly increases the complexity of equipment pipelines and control, and the overall footprint of the device is large. In order to overcome these defects, the development of high-efficiency, low-energy consumption, and low-cost CO2 separation technologies (such as adsorption and membrane separation) has become a research hotspot in this field. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of small CO2 adsorption working capacity, poor selectivity and insufficient carbon chemical adsorption and desorption of organic amine aqueous solution in the prior art adsorbents such as silica gel, activated carbon, alumina and other porous carbon-based and metal-based adsorbents, and to provide a SiO2 aerogel and a preparation method and application thereof. The SiO2 aerogel has the characteristics of low density, large specific surface area, high porosity, excellent adsorption and regeneration performance, and the preparation method is low-cost and convenient process.

[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a SiO2 aerogel, wherein the SiO2 aerogel is a SiO2 aerogel loaded with a complex amine;

[0006] The pore volume of the SiO2 aerogel is 0.8-1.5cm 3 / g, with a specific surface area of ​​200-850m 2 / g, porosity 75-99.5%;

[0007] The SiO2 aerogel has a SiO2 skeleton volume fraction of less than 10%, and a three-dimensional grid void volume fraction of greater than or equal to 90%.

[0008] A second aspect of the present invention provides a method for preparing SiO2 aerogel, wherein the preparation method comprises the following steps:

[0009] (1) impregnating SiO2 alcohol gel with a composite amine solution, soaking it in water after impregnation equilibrium, and drying it to obtain a pre-ultrasonicated SiO2 aerogel;

[0010] (2) contacting the pre-ultrasonicated SiO2 aerogel in step (1) with water under ultrasonic and nitrogen purge conditions to obtain a transparent colloid;

[0011] (3) Aging the transparent colloid to obtain the SiO2 aerogel.

[0012] The third aspect of the present invention provides a SiO2 aerogel prepared by the above preparation method.

[0013] The fourth aspect of the present invention provides an application of the SiO2 aerogel provided in the first and third aspects in carbon dioxide capture. Through the above technical solution, the SiO2 aerogel provided by the present invention and its preparation method and application obtain the following beneficial effects:

[0014] The SiO2 aerogel provided by the present invention has the characteristics of low density, large specific surface area, high porosity, excellent adsorption and regeneration performance and can be recycled for many times. The preparation method of the SiO2 aerogel modifies the surface of the SiO2 aerogel with complex amine by ultrasonic impregnation. The preparation method has low cost and convenient process.

[0015] Furthermore, the SiO2 aerogel described in the present invention has important promotion value for solving the high regeneration energy consumption problem commonly existing in existing chemical absorption technology, reducing thermal degradation caused by high-temperature regeneration, and achieving high efficiency, miniaturization and modularization of carbon dioxide absorption modules. DETAILED DESCRIPTION

[0016] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0017] The first aspect of the present invention provides a SiO2 aerogel, wherein the SiO2 aerogel is a complex amine-loaded SiO2 aerogel;

[0018] The pore volume of the SiO2 aerogel is 0.8-1.5cm 3 / g, with a specific surface area of ​​200-850m 2 / g, porosity 75-99.5%;

[0019] The SiO2 aerogel has a SiO2 skeleton volume fraction of less than 10%, and a three-dimensional grid void volume fraction of greater than or equal to 90%.

[0020] According to the present invention, preferably, the pore volume of the SiO2 aerogel is 1.2-1.5 cm 3 / g, specific surface area of ​​500-850m 2 / g, and the porosity is 85-99.5%.

[0021] According to the present invention, in one embodiment of the present invention, the pore volume of the SiO2 aerogel is 1.35-1.5 cm 3 / g, specific surface area is 700-850m 2 / g, and the porosity is 90-99.5%.

[0022] In the present invention, the porosity is the percentage of the internal pore volume of the SiO2 aerogel to its overall volume, the internal pore volume of the SiO2 aerogel is the total volume occupied by the pores in the SiO2 aerogel, and the overall volume is the total volume of the SiO2 aerogel. That is, the porosity is the volume percentage of the pores in the porous structure of the SiO2 aerogel.

[0023] According to the present invention, the SiO2 skeleton volume fraction of the SiO2 aerogel is less than 8%, and the three-dimensional grid void volume fraction is greater than or equal to 92.5%.

[0024] In the present invention, the SiO2 aerogel is in the form of particles, and the three-dimensional grid void volume fraction is the percentage of the void volume between particles in the SiO2 aerogel to its stacking volume. That is, the three-dimensional grid void volume fraction characterizes the proportion of the void part between particles in the stacking space formed by the stacking of multiple SiO2 aerogel particles.

[0025] According to the present invention, the loading amount of the composite amine accounts for 30-80% of the mass of the SiO2 aerogel.

[0026] According to the present invention, the density of the SiO2 aerogel is 0.001-0.5 g / cm 3 .

[0027] According to the present invention, preferably, the density of the SiO2 aerogel is 0.001-0.28 g / cm 3 .

[0028] A second aspect of the present invention provides a method for preparing SiO2 aerogel, wherein the preparation method comprises the following steps:

[0029] (1) impregnating SiO2 alcohol gel with a composite amine solution, soaking it in water after impregnation equilibrium, and drying it to obtain a pre-ultrasonicated SiO2 aerogel;

[0030] (2) contacting the pre-ultrasonicated SiO2 aerogel in step (1) with water under ultrasonic and nitrogen purge conditions to obtain a transparent colloid;

[0031] (3) Aging the transparent colloid to obtain the SiO2 aerogel.

[0032] During the research process of the present invention, the inventors found that according to the preparation method of the above-mentioned specific mixed impregnation and ultrasound and the above-mentioned other steps in combination, the complex amine is modified in the mesopores of SiO2 aerogel, so that the prepared SiO2 aerogel has the characteristics of low density, large specific surface area, high porosity, excellent adsorption and regeneration performance and can be recycled many times, and the preparation method is low-cost and the process is convenient.

[0033] In the present invention, the purpose of immersing in water is to remove the residual unmodified complex amine on the SiO2 alcohol gel.

[0034] In the present invention, the purpose of nitrogen purging is to eliminate the influence of diffusion outside the system. The diffusion outside the system is the process in which the reactant molecules (CO2) reach the outer surface of the particles from the fluid phase through the stationary gas film (or liquid film) attached to the gas-solid boundary layer, or the product molecules enter the fluid phase from the outer surface of the particle through the stationary layer.

[0035] According to the present invention, the immersion temperature is 30-80° C., and the immersion time is 0.5-3 h.

[0036] According to the present invention, the soaking time is 1-3 hours, preferably 2-2.5 hours.

[0037] According to the present invention, the drying temperature is 60-120° C., and the drying time is 3-12 hours.

[0038] According to the present invention, the mass ratio of the alcohol gel to the complex amine solution is 1:1.5-5.

[0039] According to the present invention, preferably, the ultrasonic conditions include: an ultrasonic frequency of 10-100 kHz, preferably 20-50 kHz; an acoustic intensity of 5 W·cm -2 -25W·m -2 , preferably 5 W·cm -2 -10W·m -2 ; Ultrasonic irradiation time is 3-15h.

[0040] In a specific embodiment of the present invention, the ultrasonic conditions include: an ultrasonic frequency of 20-50 kHz; an acoustic intensity of 5 W·cm -2 -10W·m -2 ; Ultrasonic irradiation time is 5-12h.

[0041] According to the present invention, preferably, the nitrogen purge rate is 100-300 mL / min, preferably 150-200 mL / min.

[0042] According to the present invention, the drying temperature is 60-120° C., and the drying time is 3-12 hours.

[0043] According to the present invention, the mass ratio of water to the alcohol gel complex amine impregnation solution is 1:1-10.

[0044] In a specific embodiment of the present invention, the mass ratio of water to the alcohol gel complex amine impregnation solution is 1:2-5.

[0045] According to the present invention, the contact temperature is 30-120° C., and the contact time is 2-24 hours.

[0046] According to the present invention, the aging temperature is 20-40° C., and the aging time is 18-24 hours.

[0047] According to the present invention, the complex amine solution comprises: a complex amine and a solvent;

[0048] According to the present invention, the complex amine is selected from at least two of monoethanolamine, diethanolamine, triethanolamine, tetraethylenepentanediamine, triethylenetetramine, N-methylmonoethanolamine, N-methyldiethanolamine, caprolactam, 2-amino-2-methyl-1-propanol, diisopropanolamine, diazabicyclo, hydroxyethylpiperazine, and morpholine.

[0049] In a specific embodiment of the present invention, the complex amine contains monoethanolamine and another amine selected from diethanolamine, triethanolamine, tetraethylenepentanediamine, triethylenetetramine, N-methylmonoethanolamine, N-methyldiethanolamine, caprolactam, 2-amino-2-methyl-1-propanol, diisopropanolamine, diazabicyclo, hydroxyethylpiperazine or morpholine.

[0050] More preferably, in the present invention, the mass ratio of monoethanolamine:the other amine is 0.5-2:1.

[0051] According to the present invention, the solvent is selected from at least one of water, non-aqueous solvent and amino acid salt solvent.

[0052] According to the present invention, the non-aqueous solvent is selected from at least one of N-formylmorpholine, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.

[0053] According to the present invention, the amino acid salt solvent is selected from at least one of glycine, sarcosine, lysine, alanine, glutamate, serine, aminoacetate, proline, arginine and histidine.

[0054] In a specific embodiment of the present invention, the mass ratio of the complex amine to the solvent is 1-9:1.

[0055] In a specific embodiment of the present invention, the complex amine solution is selected from the following complex amine solutions:

[0056] Composite amine solution-1: the composite amine is monoethanolamine and diazabicyclic, and the solvent is water; wherein the mass ratio of monoethanolamine to diazabicyclic is 1-2:1;

[0057] Composite amine solution-2: the composite amine is monoethanolamine and 2-amino-2-methyl-1-propanol, and the solvent is N,N-dimethylacetamide; wherein the mass ratio of monoethanolamine to 2-amino-2-methyl-1-propanol is 0.75-1.5:1;

[0058] Composite amine solution-3: the composite amine is monoethanolamine and tetraethylenepentanediamine, the solvent is sodium sarcosinate, and the mass ratio of monoethanolamine to tetraethylenepentanediamine is 1.5-2:1.

[0059] In the present invention, the composite amine is modified into the pores of SiO2 aerogel, so that the SiO2 aerogel has the advantages of both absorption and adsorption methods, so as to achieve the purpose of increasing the adsorption amount and selectivity of CO2.

[0060] According to the present invention, the concentration of the complex amine solution is 1-5 mol / L, and the concentration is the concentration of the complex amine.

[0061] In a specific embodiment of the present invention, the concentration of the complex amine solution is 3-5 mol / L.

[0062] In the present invention, the pore structure material of SiO2 aerogel prepared by using the complex amine solution in the above concentration range has uniform pore size distribution, high specific surface area and specific pore volume, which can promote the uniform dispersion of amine groups and greatly increase the contact area between amine groups and gas phase, thereby increasing mass transfer and reaction rate and improving the utilization rate of the complex amine.

[0063] In the present invention, the alcohol gel is prepared by a conventional method, and a specific preparation method is provided below:

[0064] Under stirring conditions, ethanol is dripped into the sol to obtain a wet gel, which is then soaked in ethanol at 40-60°C, with the ethanol replaced every 24 hours for 48 hours, then soaked in a mixture of tetraethyl orthosilicate and ethanol for 48 hours, and finally soaked in ethanol, with the ethanol replaced every 24 hours for 48 hours.

[0065] The third aspect of the present invention provides a SiO2 aerogel prepared by the above preparation method.

[0066] In the present invention, since SiO2 aerogel has a pore structure material with a large pore volume and a skeleton structure with good open connectivity, it can carry more organic amines and thus provide more adsorption active sites, thereby having higher carbon dioxide adsorption performance, adsorption rate and selectivity.

[0067] The fourth aspect of the present invention provides an application of the SiO2 aerogel provided in the first and third aspects for carbon dioxide capture.

[0068] The present invention will be described in detail below by way of examples. In the following examples,

[0069] The CO2 adsorption and desorption performance of SiO2 aerogel was tested by the classic dynamic adsorption process:

[0070] The reaction system consists of simulated flue gas, a flow meter, a water saturator, a heating pipeline, an adsorption column, a complex amine aerogel adsorbent, a thermocouple, a heating furnace and a gas chromatograph.

[0071] The dynamic adsorption test of SiO2 aerogel on CO2 was carried out in a fixed bed adsorber. The fixed bed reactor used a glass adsorption column, and the temperature of the adsorption column was controlled by a heating furnace. The humidity of the reaction gas was controlled by a water saturator. During the adsorption process, 5.0g of SiO2 aerogel was filled in the adsorption column, and a dry carbon dioxide / nitrogen mixed gas passed through the pipeline at a flow rate of 50mL / min. The gas flow was controlled by an electronic flowmeter. The carbon dioxide concentration of the inlet and outlet gas was determined using a gas chromatograph equipped with a thermal conductivity detector (TCD). The CO2 content in the raw gas was 12.5wt%, and the remaining gas was supplemented with N2.

[0072] The raw materials used in the examples and comparative examples are all commercially available.

[0073] The porosity is calculated by the following formula:

[0074] ρ1=m / v;

[0075] Porosity = (1-ρ1 / ρ0) × 100%;

[0076] Among them, m is the mass of aerogel, v is the volume of aerogel particles themselves, ρ1 is the apparent density of aerogel particles, and ρ0 is the theoretical density of silica.

[0077] The void volume fraction of the three-dimensional grid is calculated by the following formula:

[0078] The void volume fraction of the three-dimensional grid = (1-ρ a / ρ1)×100%;

[0079] Among them, ρ a is the packing density, which is the mass of all aerogel particles in the packing space / the total volume of the packing space.

[0080] Example 1

[0081] The preparation method of SiO2 aerogel comprises the following steps:

[0082] (1) Place 20% alkaline silica gel in a beaker and stir at a rate of 150 r / min. Use 0.8 mol / L hydrochloric acid to adjust the pH value of the silica sol dispersion. Slowly drip an appropriate amount of ethanol into the dispersion and keep it at a constant temperature of 60°C for 8 hours to obtain a wet gel. Then put the wet gel into ethanol and soak it at a constant temperature of 60°C for 24 hours. After two consecutive soakings, soak it in a mixture of tetraethyl orthosilicate (TEOS) and ethanol for 48 hours, and then continue to soak it in ethanol for 24 hours, and soak it twice in succession to replace and remove the moisture in the wet gel.

[0083] (2) The prepared alcohol gel was then added with 30 g of a 2.0 mol / L composite amine-1 solution, the composition of which was: monoethanolamine (30 wt%), diazabicyclo (20 wt%) and deionized water (50

[0084] wt%). Stir at 150r / min for 30min at 60℃. Soak in water for 2h and dry at 90℃ for 6h. Turn on 30kHz horn type ultrasound, add distilled water, and the ultrasound intensity is 5.0

[0085] W / cm 2 , maintaining the temperature at 80°C, the ultrasonic irradiation time for 12 h, and the nitrogen purge rate at 200 mL / min to generate a transparent colloid.

[0086] (3) The colloid was aged at room temperature to obtain composite amine SiO2 aerogel A1. The performance parameters of A1 are shown in Table 2.

[0087] Example 2

[0088] The method of Example 1 was followed, except that the concentration of the complex amine solution-1 was 3.0 mol / L, to obtain complex amine SiO2 aerogel A2. The performance parameters of A2 are shown in Table 2.

[0089] Example 3

[0090] The method of Example 1 was followed, except that the concentration of the composite amine solution-1# was 4.0 mol / L, to obtain composite amine SiO2 aerogel A3. The performance parameters of A3 are shown in Table 2.

[0091] Example 4

[0092] The method of Example 1 is followed, except that the complex amine solution is complex amine solution-2, and its formula composition is: monoethanolamine (30wt%), 2-amino-2-methyl-1-propanol (40wt%) and N,N-dimethylacetamide (30wt%), to obtain complex amine SiO2 aerogel A4, and the performance parameters of A4 are shown in Table 2.

[0093] Example 5

[0094] The method of Example 4 was followed, except that the concentration of the complex amine solution-2 was 3.0 mol / L, to obtain complex amine SiO2 aerogel A5. The performance parameters of A5 are shown in Table 2.

[0095] Example 6

[0096] The method of Example 4 was followed, except that the concentration of the complex amine solution-2 was 4.0 mol / L, to obtain complex amine SiO2 aerogel A6. The performance parameters of A6 are shown in Table 2.

[0097] Example 7

[0098] The method of Example 1 is followed, except that the composite amine solution is composite amine solution-3, which is composed of: monoethanolamine (40wt%), tetraethylenepentanediamine (20wt%) and sodium sarcosinate (40wt%), to obtain composite amine SiO2 aerogel A7, and the performance parameters of A7 are shown in Table 2.

[0099] Example 8

[0100] The method of Example 7 was followed, except that the concentration of the complex amine solution-3 was 3.0 mol / L, to obtain complex amine SiO2 aerogel A8. The performance parameters of A8 are shown in Table 2.

[0101] Example 9

[0102] The method of Example 7 was followed, except that the concentration of the complex amine solution-3 was 4.0 mol / L, to obtain complex amine SiO2 aerogel A9. The performance parameters of A9 are shown in Table 2.

[0103] Comparative Example 1

[0104] The method of Example 1 is followed, except that step (2) is not performed under ultrasonic conditions, to obtain composite amine SiO2 aerogel D1. The performance parameters of D1 are shown in Table 2.

[0105] Comparative Example 2

[0106] The method of Example 1 was followed, except that the impregnation was carried out under ultrasonic conditions and no ultrasonic treatment was performed after the impregnation to obtain the composite amine SiO2 aerogel D2. The performance parameters of D2 are shown in Table 2.

[0107] Comparative Example 3

[0108] The method of Example 1 was followed, except that the immersion temperature was 25° C. and the immersion time was 0.25 h, to obtain composite amine SiO2 aerogel D3. The performance parameters of D3 are shown in Table 2.

[0109] Comparative Example 4

[0110] The method of Example 1 was followed, except that the ultrasonic frequency was 120 kHz and the sound intensity was 35 W·m -2 , the ultrasonic irradiation time is 18h, and the composite amine SiO2 aerogel D4 is obtained. The performance parameters of D4 are shown in Table 2.

[0111] Comparative Example 5

[0112] The method of Example 1 was followed, except that there was no nitrogen purge in step (2), to obtain composite amine SiO2 aerogel D5. The performance parameters of D5 are shown in Table 2.

[0113] Comparative Example 6

[0114] The method of Example 1 was followed, except that the solution was a 2.0 mol / L monoethanolamine solution (30 wt%), to obtain composite amine SiO2 aerogel D6. The performance parameters of D6 are shown in Table 2.

[0115] Material CO2 cycle adsorption-desorption performance test

[0116] A1 and D1 were subjected to 50 consecutive CO2 cycle adsorption-desorption tests, and the results are shown in Tables 3 and 4.

[0117] Table 1 shows the structural parameters of SiO2 aerogel N1 which is not loaded with complex amine by ultrasonic impregnation, and the SiO2 aerogels of Examples 1-9 and Comparative Examples 1-6.

[0118] Table 1

[0119]

[0120]

[0121] Table 2

[0122] serial number <![CDATA[Adsorption capacity (mmol CO2 / g adsorbent)]]> Desorption rate (%) <![CDATA[CO2 content of the regeneration gas (%)]]> Example 1 4.8 80 97.5 Example 2 5.2 88 99.3 Example 3 5.1 85 99.0 Example 4 5.2 92 99.3 Example 5 6.0 96 99.9 Example 6 5.6 95 99.5 Example 7 4.9 86 97.8 Example 8 5.3 91 98.3 Example 9 5.2 90 97.3 Comparative Example 1 3.8 75 95.2 Comparative Example 2 4.0 73 93.0 Comparative Example 3 3.2 65 85.2 Comparative Example 4 3.9 70 87.6 Comparative Example 5 4.5 76 93.8 Comparative Example 6 4.6 78 94.2

[0123] Table 3

[0124]

[0125]

[0126] Table 4

[0127]

[0128] It can be seen from Table 1 that the pore volume, specific surface area, porosity and density of the aerogels prepared in Examples 1-9 of the present invention have changed. It can be seen from the results of Table 2 that the aerogels prepared in Examples 1-9 of the present invention have higher CO2 adsorption, desorption rate and regeneration gas CO2 content. Compared with Examples 1, 4 and 7, Examples 2-3, 5-6 and 8-9 have higher CO2 adsorption, desorption rate and regeneration gas CO2 content, respectively, indicating that the adsorption and desorption performance of the aerogel can be significantly increased when the concentration of the composite amine solution is 3-5 mol / L. Compared with the comparative example, the aerogel prepared by the preparation method of the present invention has a specific pore volume, specific surface area, porosity, three-dimensional grid void volume fraction, density and composite amine loading, so that its CO2 adsorption, desorption rate and regeneration gas CO2 content are higher. In addition, compared with conventional adsorbents (3.0-4.0mmol CO2 / g adsorbent), the adsorption capacity of the SiO2 aerogel is increased by more than 20%.

[0129] By comparing Table 3 and Table 4, it can be seen that after the SiO2 aerogel provided by the present invention has gone through 50 continuous cycles of adsorption-desorption of CO2, the decrease in the adsorption amount of the SiO2 aerogel is less than 5% of the initial adsorption amount; and after D1 has gone through 50 continuous cycles of adsorption-desorption of CO2, the decrease in the adsorption capacity of the SiO2 aerogel is 40% of the initial adsorption amount, indicating that the SiO2 aerogel provided by the present invention has excellent CO2 cyclic adsorption-desorption performance.

[0130] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A SiO2 aerogel, characterized in that: The SiO2 aerogel is a SiO2 aerogel loaded with complex amine; The pore volume of the SiO2 aerogel is 0.8-1.5cm 3 / g, with a specific surface area of ​​200-850m 2 / g, porosity 75-99.5%; The SiO2 aerogel has a SiO2 skeleton volume fraction of less than 10%, and a three-dimensional grid void volume fraction of greater than or equal to 90%.

2. The SiO2 aerogel according to claim 1, wherein The SiO2 aerogel has a SiO2 skeleton volume fraction of less than 8%, and a three-dimensional grid void volume fraction of greater than or equal to 92.5%; Preferably, the composite amine loading accounts for 30-80% of the mass of the SiO2 aerogel.

3. The SiO2 aerogel according to claim 1 or 2, wherein: The density of the SiO2 aerogel is 0.001-0.5 g / cm 3 ; Preferably, the density of the SiO2 aerogel is 0.001-0.28 g / cm 3 .

4. A method for preparing SiO2 aerogel, characterized in that: The preparation method comprises the following steps: (1) impregnating SiO2 alcohol gel with a composite amine solution, soaking it in water after impregnation equilibrium, and drying it to obtain a pre-ultrasonicated SiO2 aerogel; (2) contacting the pre-ultrasonicated SiO2 aerogel in step (1) with water under ultrasonic and nitrogen purge conditions to obtain a transparent colloid; (3) Aging the transparent colloid to obtain the SiO2 aerogel.

5. The preparation method according to claim 4, wherein: The immersion temperature is 30-80°C, and the immersion time is 0.5-3h; Preferably, the soaking time is 1-3 hours, preferably 2-2.5 hours; Preferably, the drying temperature is 60-120°C, and the drying time is 3-12h; Preferably, the mass ratio of the SiO2 alcohol gel to the complex amine solution is 1:1.5-5; Preferably, the ultrasonic conditions include: an ultrasonic frequency of 10-100 kHz, preferably 20-50 kHz; an acoustic intensity of 5 W·cm -2 -25W·m -2 , preferably 5 W·cm -2 -10W·m -2 ; Ultrasonic irradiation time is 3-15h; Preferably, the nitrogen purge rate is 100-300 mL / min, preferably 150-200 mL / min; Preferably, the mass ratio of water to SiO2 alcohol gel composite amine impregnation liquid is 1:1-10, preferably 1:2-5; Preferably, the contact temperature is 30-120°C, and the contact time is 2-24h; Preferably, the aging temperature is 20-40° C., and the aging time is 18-24 h.

6. The preparation method according to claim 4 or 5, wherein: The complex amine solution comprises: complex amine and solvent; Wherein, the composite amine is selected from at least two of monoethanolamine, diethanolamine, triethanolamine, tetraethylenepentanediamine, triethylenetetramine, N-methylmonoethanolamine, N-methyldiethanolamine, caprolactam, 2-amino-2-methyl-1-propanol, diisopropanolamine, diazabicyclo, hydroxyethylpiperazine, and morpholine; preferably, the composite amine contains monoethanolamine and another amine selected from diethanolamine, triethanolamine, tetraethylenepentanediamine, triethylenetetramine, N-methylmonoethanolamine, N-methyldiethanolamine, caprolactam, 2-amino-2-methyl-1-propanol, diisopropanolamine, diazabicyclo, hydroxyethylpiperazine, or morpholine; preferably, the mass ratio of monoethanolamine to the another amine is 0.5-2:1; Preferably, the solvent is selected from at least one of water, non-aqueous solvent, and amino acid salt solvent; Preferably, the non-aqueous solvent is selected from at least one of N-formylmorpholine, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone; Preferably, the amino acid salt solvent is selected from at least one of glycine, sarcosine, lysine, alanine, glutamate, serine, aminoacetate, proline, arginine, and histidine; Preferably, the mass ratio of the complex amine to the solvent is 1-9:

1.

7. The preparation method according to claim 6, wherein The complex amine solution is selected from the following complex amine solutions: Composite amine solution-1: the composite amine is monoethanolamine and diazabicyclic, the solvent is water, wherein the mass ratio of monoethanolamine to diazabicyclic is 1-2:1; Composite amine solution-2: the composite amine is monoethanolamine and 2-amino-2-methyl-1-propanol, the solvent is N,N-dimethylacetamide, wherein the mass ratio of monoethanolamine to 2-amino-2-methyl-1-propanol is 0.75-1.5:1; Composite amine solution-3: the composite amine is monoethanolamine and tetraethylenepentanediamine, the solvent is sodium sarcosinate, and the mass ratio of monoethanolamine to tetraethylenepentanediamine is 1.5-2:

1.

8. A method according to any one of claims 4 to 7, wherein The concentration of the complex amine solution is 1-5 mol / L, preferably 3-5 mol / L.

9. A SiO2 aerogel prepared by the preparation method according to any one of claims 4 to 8.

10. Use of the SiO2 aerogel according to any one of claims 1 to 3 and 9 in carbon dioxide capture.