Catalyst for preparing aviation kerosene distillate oil from carbon dioxide-rich synthesis gas as well as preparation method and application of catalyst
Through the preparation of composite metal oxide catalysts and the use of microwave heating and calcining technology, the problem of insufficient conversion and selectivity of existing catalysts in carbon dioxide-rich synthesis gas is solved, and efficient CO conversion and low CO2 selectivity meets the aviation industry's demand for green aviation coal.
Patent Information
- Application Number
- CN202411001702.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The conversion and selectivity of existing catalysts to make aviation kerosene distillates by hydrogenating in carbon dioxide-rich synthesis gas is insufficient, and it is difficult to effectively reduce the selectivity of CO2, which cannot meet the aviation industry's demand for green aviation coal.
Using composite metal oxide catalysts, including Fe 40%-70%, Mn 5%-20%, K 5%-20%, and K 5%-20%, prepared by preparing a precursor solution containing iron, manganese and potassium and adding organic matter to microwave heating and calculating. Catalysts with high CO conversion and low CO2 selectivity are produced.
It significantly improves the conversion rate of carbon dioxide-rich synthesis gas and the selectivity of aviation kerosene fractions, while reducing the selectivity of CO2, making it simple in process and high efficiency, and is suitable for large-scale industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a catalyst for preparing aviation kerosene fraction from carbon dioxide-rich synthesis gas, and a preparation method and application thereof. Background Art
[0002] The main components of aviation kerosene are long-chain hydrocarbons, with a typical carbon chain length distribution of C8-C 18 , where the ideal carbon chain length is C8-C 16 . In the current energy structure, hydrocarbon liquid fuels derived from petroleum play an extremely important role. However, petroleum resources are non-renewable, while people's demand for hydrocarbon liquid fuels is increasing day by day, and petroleum resources will eventually be exhausted. Although electric vehicles have begun to become popular, for the aviation industry that flies long distances, due to its stringent requirements for energy and power density, aviation kerosene is difficult to be replaced by electric energy storage technology now and in the future. At this stage, there is no choice but liquid fuel.
[0003] Jet fuel is currently recognized by the world's aviation industry as a feasible route to reduce CO2 emissions, such as converting CO2 into CO or gasifying biomass to obtain synthesis gas, and then synthesizing jet fuel through the Fischer-Tropsch synthesis reaction. The rapidly developing aviation industry urgently needs a large amount of green jet fuel as a clean power source. Therefore, how to obtain green jet fuel with high selectivity and low cost has become an international academic hotspot and an industry pain point.
[0004] The Fischer-Tropsch synthesis reaction can convert synthesis gas into high-quality liquid fuels and high-value chemicals such as low-carbon olefins and high-quality paraffin under the action of a catalyst. The liquid fuel generated by the Fischer-Tropsch synthesis route has the characteristics of being sulfur-free and nitrogen-free, and is an environmentally friendly fuel. Iron-based catalysts are one of the main Fischer-Tropsch synthesis catalysts and a hot topic in the research of Fischer-Tropsch synthesis catalysts. Due to their low price, they also have the advantage of achieving large-scale industrialization. Chinese patent application CN103611537A reports an iron-based Fischer-Tropsch synthesis catalyst and its preparation method and application. The iron-based catalyst reduces the selectivity of carbon dioxide while increasing the conversion rate of synthesis gas. Chinese patent application CN105013486A reports a preparation method and application of a core-shell structured Fe3O4@C catalyst for Fischer-Tropsch synthesis, which has high Fischer-Tropsch synthesis activity and C 5+ Chinese patent CN1199730C reports a Fischer-Tropsch synthesis iron / manganese catalyst and its preparation method, which has high catalyst activity, low carbon olefins and C 5+ The catalyst has the advantages of good selectivity, low methane selectivity, etc. At present, there is no report on the catalyst for preparing aviation kerosene fraction by hydrogenation of carbon dioxide-rich synthesis gas with high selectivity, its preparation method and application.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide a catalyst for the hydrogenation of carbon dioxide-rich synthesis gas to produce aviation kerosene distillate oil. The catalyst can effectively improve the CO conversion rate and the selectivity of the aviation kerosene distillate, and at the same time can significantly reduce the selectivity of CO2. It can be used for the catalytic hydrogenation of carbon dioxide-rich synthesis gas to prepare aviation kerosene distillate oil with high selectivity.
[0007] The second object of the present invention is to provide a method for preparing the catalyst as described above, which has the advantages of simple process, effective control of the catalyst component content, good repeatability, etc., and can improve efficiency and catalyst activity through microwave heating and drying.
[0008] The third object of the present invention is to provide a use of the catalyst as described above in the preparation of aviation kerosene distillate from carbon dioxide-rich synthesis gas.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] A catalyst for preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas, the catalyst being a composite metal oxide, comprising, by mass percentage, 40%-70% of Fe, 5%-20% of Mn, 5%-20% of K and the remainder of O; when the catalyst is used for the reaction of hydrogenating carbon dioxide-rich synthesis gas to prepare aviation kerosene distillate, the CO conversion rate is greater than 55%, the CO2 selectivity is less than 30%, and the C8-C 16 The selectivity to hydrocarbon products is >37%.
[0011] The method for preparing the catalyst described in the above embodiment comprises the following steps:
[0012] (1) preparing a precursor solution containing iron, manganese and potassium;
[0013] (2) adding organic matter to the precursor solution described in step (1) and mixing;
[0014] (3) The mixed solution in step (2) is subjected to microwave heating and calcination to obtain the catalyst.
[0015] The catalyst described in the above embodiments is used in the preparation of aviation kerosene distillate from carbon dioxide-rich synthesis gas.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The catalyst of the present invention can be applied to the reaction of preparing aviation kerosene fraction from synthesis gas containing a certain concentration of carbon dioxide by regulating the active sites and optimizing the reaction conditions, and can effectively improve the conversion rate of carbon dioxide-rich synthesis gas and the selectivity of aviation kerosene fraction, and can reduce the selectivity of carbon dioxide.
[0018] (2) The method of the present invention can accurately control the chemical composition of each component of the catalyst by adjusting the ratio of metal precursor salt and organic matter, and has good repeatability. In addition, the method uses microwave heating. Compared with traditional heating methods, it has the advantages of fast and simple preparation process, uniform heating, low energy consumption, and easy industrial scale-up, which can effectively improve the preparation efficiency and catalytic performance of the catalyst. DETAILED DESCRIPTION
[0019] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0020] The first aspect of the present invention provides a catalyst for preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas, wherein the catalyst is a composite metal oxide, which comprises, by mass percentage, 40%-70% of Fe, 5%-20% of Mn, 5%-20% of K and the remainder of O; when the catalyst is used for the reaction of hydrogenating carbon dioxide-rich synthesis gas to prepare aviation kerosene distillate, the CO conversion rate is greater than 55%, the CO2 selectivity is less than 30%, and the C8-C 16 The selectivity to hydrocarbon products is >37%.
[0021] In some embodiments of the present invention, typically but not limiting, for example, the mass percentage of Fe element in the catalyst can be 40%, 50%, 60% or 70%, or other values within the range; the mass percentage of Mn element in the catalyst can be 5%, 10%, 15% or 20%, or other values within the range; the mass percentage of K element in the catalyst can be 5%, 10%, 15% or 20%, or other values within the range. When the catalyst is used for the reaction of hydrogenating carbon dioxide-rich synthesis gas to produce aviation kerosene distillate, typically but not limiting, for example, the CO conversion rate can be 55.8%, 56.1%, 61.3%, 62.3%, 64.2% or 67.3%, or other values within the range; CO2 selectivity can be 29.4%, 28.3%, 25.5%, 24% or 22.5%, or other values within the range; C8-C 16 The selectivity to hydrocarbon products may be 37.3%, 39.2%, 51.1%, 54.3%, 57.1%, or 60.8%, or other values within a range.
[0022] The catalyst provided by the present invention can be applied to the reaction of hydrogenating synthesis gas containing a certain concentration of carbon dioxide to produce aviation kerosene fractions, and can significantly improve the conversion rate of carbon dioxide-rich synthesis gas and the selectivity of aviation kerosene fractions, while significantly reducing the selectivity of CO2.
[0023] The second aspect of the present invention provides a method for preparing the catalyst described in the aforementioned embodiment, comprising the following steps:
[0024] (1) preparing a precursor solution containing iron, manganese and potassium;
[0025] (2) adding organic matter to the precursor solution described in step (1) and mixing;
[0026] (3) The mixed solution in step (2) is subjected to microwave heating and calcination to obtain the catalyst.
[0027] The method of the present invention has a simple preparation process, can effectively control the content of catalyst components, has good repeatability, is convenient for large-scale production, adopts microwave heating, quickly heats up through internal friction, heats the inside and outside of the solution simultaneously, does not require any heat conduction process, has a fast and uniform heating speed, and can effectively improve the preparation efficiency and catalytic performance of the catalyst.
[0028] In some specific embodiments of the present invention, in step (1), the method for preparing a precursor solution containing iron, manganese and potassium comprises the following steps:
[0029] The iron source, manganese source and potassium source (precursors of iron, manganese and potassium) are mixed with a solvent to obtain the product.
[0030] In some specific embodiments of the present invention, in step (1), the mixing is stirring mixing, and the stirring mixing conditions are not specifically limited, and are based on the complete dissolution of the iron source, manganese source and potassium source. In some embodiments, the stirring mixing time can be 1-2h.
[0031] In some specific embodiments of the present invention, in step (1), the iron source used to prepare the precursor solution is a soluble iron salt, for example, it may include one or more of iron nitrate, sulfate and chloride.
[0032] In some specific embodiments of the present invention, in step (1), the manganese source used to prepare the precursor solution is a soluble manganese salt, for example, it may include one or more of manganese nitrate, sulfate and chloride.
[0033] In some specific embodiments of the present invention, in step (1), the potassium source used to prepare the precursor solution is a soluble potassium salt, for example, it may include one or more of potassium nitrate, sulfate and chloride.
[0034] In some specific embodiments of the present invention, in step (1), the solvent used to prepare the precursor solution includes water. To avoid impurities, the water is preferably deionized water.
[0035] In some specific embodiments of the present invention, in step (1), the total concentration of the three metal elements iron, manganese and potassium in the precursor solution is 0.1-3.0 mol / L. Typically but not restrictively, the total concentration of iron, manganese and potassium can be 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L or 3 mol / L, or other values within the range.
[0036] In some specific embodiments of the present invention, in step (2), the organic matter includes one or more of urea, citric acid, oxalic acid, and tartaric acid. The organic matter plays a role of combustion during the roasting process and also plays a role of dispersing metals.
[0037] In some preferred embodiments of the present invention, the organic matter is tartaric acid, and when the prepared catalyst is used for hydrogenation of carbon dioxide-rich synthesis gas to produce aviation kerosene distillate, the CO conversion rate can reach 67.3%, and the C8-C 16 The selectivity of hydrocarbon products can reach 60.8%, and the CO2 selectivity can be reduced to 22.5%.
[0038] In some specific embodiments of the present invention, in step (2), the concentration of organic matter in the mixed solution is 0.2-6.0 mol / L, for example, it can be 0.2 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L or 6 mol / L, or other values within the range.
[0039] In some specific embodiments of the present invention, in step (2), the mixing is stirring mixing, which is carried out under water bath heating conditions, the stirring time is 1-4 hours, and the heating temperature is 30-80°C. The purpose of stirring and water bath heating is to accelerate dissolution. Typically but not restrictive, for example, the stirring time can be 1 hour, 2 hours, 3 hours or 4 hours, and can also be other values within the range; the heating temperature can be 30°C, 40°C, 50°C, 60°C, 70°C or 80°C, and can also be other values within the range.
[0040] In some specific embodiments of the present invention, in step (3), the power of microwave heating is 200-800 W, the time is 10-30 min, and the stirring speed is 200-1000 rpm; typically but not limiting, for example, the power of microwave heating can be 200 W, 400 W, 500 W, 600 W or 800 W, or other values within the range; the time of microwave heating can be 10 min, 15 min, 20 min, 25 min or 30 min, or other values within the range; the stirring speed can be 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm, or other values within the range.
[0041] The traditional heating method takes a long time, consumes a lot of energy, and the heating process is uneven. The present invention uses microwave heating to dry, which can heat the inside and outside at the same time, making the heating more uniform and the heating speed faster. Within a certain heating power range (200-800w), the performance of the catalyst can be significantly improved.
[0042] In some specific embodiments of the present invention, in step (3), the calcination temperature is 300-400°C, and the calcination time is 2-6h; typically but not limiting, for example, the calcination temperature can be 300°C, 320°C, 350°C, 380°C or 400°C, or other values within the range; the calcination time can be 2h, 3h, 4h, 5h or 6h, or other values within the range.
[0043] The third aspect of the present invention provides a catalyst as described in the aforementioned embodiment, or a catalyst prepared by the preparation method as described in any one of the aforementioned embodiments, for use in preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas, wherein the volume ratio of CO2 to (CO+CO2) in the carbon dioxide-rich synthesis gas is 1-5:10, and the volume ratio of H2 to (CO+CO2) is 1-3:1;
[0044] And / or, the reaction temperature for preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas is 280-360°C, the reaction pressure is 2.0-5.0MPa, and the reaction space velocity is 1000-15000h-1 .
[0045] In some embodiments, typically but not limiting, for example, the volume ratio of CO2 and (CO+CO2) can be 1:10, 2:10, 3:10, 4:10 or 5:10, or other values within the range; the volume ratio of H2 and (CO+CO2) can be 1:1, 1.5:1, 2:1, 2.5:1 or 3:1, or other values within the range; the reaction temperature for preparing aviation kerosene distillate from the carbon dioxide-rich synthesis gas can be 280°C, 300°C, 320°C, 340°C or 360°C, or other values within the range; the reaction pressure can be 2.0MPa, 3.0MPa, 4.0MPa or 5.0MPa, or other values within the range; the reaction space velocity can be 1000h -1 , 2000h -1 , 4000h -1 、8000h -1 、10000h -1 、12000h -1 or 15000h -1 , or other values within the range.
[0046] In some specific embodiments of the present invention, the process of preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas comprises the following steps:
[0047] The catalyst is loaded into a fixed bed reactor, and a synthesis gas atmosphere is introduced for reduction, and then the synthesis gas rich in carbon dioxide is switched for reaction.
[0048] In some specific embodiments of the present invention, the reduction temperature is 320-380°C, and the reduction time is 16-24h. Typically but not limitatively, for example, the reduction temperature can be 320°C, 340°C, 360°C or 380°C, or other values within the range; the reduction time can be 16h, 18h, 20h, 22h or 24h, or other values within the range.
[0049] Example 1
[0050] 40.4g of Fe(NO3)3·9H2O, 1.79g of Mn(NO3)2·9H2O, and 0.69g of KNO3 were weighed and placed in a beaker, 46.6g of water was added to dissolve them, and stirred for 1 hour. 36.1g of tartaric acid was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, and then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 500W and a stirring speed of 600rpm, and then transferred to a muffle furnace and programmed to 350°C for calcination for 4 hours to obtain a catalyst.
[0051] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out.
[0052] Example 2
[0053] 40.4g of Fe(NO3)3·9H2O, 1.79g of Mn(NO3)2·9H2O, and 0.69g of KNO3 were weighed and placed in a beaker, 46.6g of water was added to dissolve them, and stirred for 1 hour. 46.1g of citric acid was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 500W and a stirring speed of 600rpm, and then transferred to a muffle furnace and programmed to 350°C for calcination for 4 hours to obtain a catalyst.
[0054] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out.
[0055] Example 3
[0056] 40.4g of Fe(NO3)3·9H2O, 1.79g of Mn(NO3)2·9H2O, and 0.69g of KNO3 were weighed and placed in a beaker, 46.6g of water was added to dissolve them, and stirred for 1 hour. 21.6g of oxalic acid was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, and then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 500W and a stirring speed of 600rpm, and then transferred to a muffle furnace and programmed to heat to 350°C and calcine for 4 hours to obtain a catalyst.
[0057] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out.
[0058] Example 4
[0059] 40.4 g of Fe(NO3)3·9H2O, 1.79 g of Mn(NO3)2·9H2O, and 0.69 g of KNO3 were weighed and placed in a beaker, 46.6 g of water was added to dissolve them, and stirred for 1 hour. 14.4 g of urea was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, and then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 500 W and a stirring speed of 600 rpm, and then transferred to a muffle furnace and programmed to rise to 350°C and calcinated for 4 hours to obtain a catalyst.
[0060] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out.
[0061] Example 5
[0062] 40.4g of Fe(NO3)3·9H2O, 1.79g of Mn(NO3)2·9H2O, and 0.69g of KNO3 were weighed and placed in a beaker, 46.6g of water was added to dissolve them, and stirred for 1 hour. 36.1g of tartaric acid was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 200W and a stirring speed of 600rpm, and then transferred to a muffle furnace and programmed to rise to 350°C and calcinated for 4 hours to obtain a catalyst.
[0063] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out.
[0064] Example 6
[0065] 40.4g of Fe(NO3)3·9H2O, 1.79g of Mn(NO3)2·9H2O, and 0.69g of KNO3 were weighed and placed in a beaker, 46.6g of water was added to dissolve them, and stirred for 1 hour. 36.1g of tartaric acid was weighed and added to the above solution, and stirred for 1 hour in a water bath at 50°C, then transferred to a porcelain crucible and heated in a microwave-assisted chemical reactor for 30 minutes, with a microwave heating power of 800W and a stirring speed of 600rpm, and then transferred to a muffle furnace and programmed to 350°C for calcination for 4 hours to obtain a catalyst.
[0066] 1.0 g of the obtained catalyst was loaded into a fixed bed reactor, and a mixed gas of CO / H2=34 / 66 (volume ratio) was introduced at 350°C for reduction for 24 hours, then the temperature was lowered to 150°C, and the raw gas was switched to CO / CO2 / H2 / N2=32 / 6 / 57 / 5 (volume ratio), and the temperature was raised to 320°C, and the mixture was heated at 2.0 MPa, 4000 h -1 The reaction was carried out below.
[0067] Comparative Example 1
[0068] The difference between Comparative Example 1 and Example 1 is that when preparing aviation kerosene distillate, after reduction with CO / H2=34 / 66 (volume ratio), the raw gas is replaced with CO / H2 / N2=38 / 57 / 5 (volume ratio), and the other conditions are the same as Example 1.
[0069] Comparative Example 2
[0070] The difference between Comparative Example 2 and Example 1 is that microwave heating is replaced by oven heating, and heating is performed at 120° C. for 12 h. The other conditions are the same as those of Example 1.
[0071] Comparative Example 3
[0072] The difference between Comparative Example 3 and Example 1 is that the catalyst is prepared by coprecipitation method, and the preparation steps are as follows:
[0073] Weigh 40.4g of Fe(NO3)3·9H2O and 1.79g of Mn(NO3)2·9H2O into beaker A, and add a certain amount of water to dissolve them. In addition, prepare 1mol / L KOH solution B. Perform co-current titration precipitation on solutions A and B, and control pH=8. After the titration, obtain precipitate C, age at 70℃ for 8 hours, centrifuge and wash 3 times, place in a 100℃ oven to dry for 12 hours, and then transfer it to a muffle furnace and program the temperature to 350℃ for calcination for 4 hours to obtain a catalyst.
[0074] The remaining conditions are the same as in Example 1.
[0075] Comparative Example 4
[0076] The difference between Comparative Example 4 and Example 1 is that no organic matter is added to the precursor solution, the precursor solution is directly heated by microwave, and the other conditions are the same as those in Example 1.
[0077] Test example
[0078] (1) The mass percentage of each element in the catalyst prepared in each embodiment and comparative example was tested by ICP. The test results are shown in Table 1.
[0079] Table 1
[0080] Fe(%) Mn(%) K(%) O(%) Example 1 42 7 8 43 Example 2 43 7 8 42 Example 3 43 6 8 43 Example 4 42 6 7 45 Example 5 43 7 8 42 Example 6 42 7 7 44 Comparative Example 1 42 7 8 43 Comparative Example 2 42 7 8 43 Comparative Example 3 44 8 8 40 Comparative Example 4 43 6 7 44
[0081] (2) In each embodiment and comparative example, after the reaction of hydrogenating the raw gas to produce aviation kerosene distillate, the reaction tail gas (including unreacted raw gas and generated gaseous products) was analyzed online by gas chromatography, and the liquid products generated by the reaction were analyzed offline by gas chromatography. The catalyst performance evaluation results are shown in Table 2.
[0082] Table 2
[0083]
[0084]
[0085] The results of catalyst performance evaluation show that the iron-manganese potassium catalyst (Example 1) obtained by using tartaric acid as an organic matter for combustion experiments has a selectivity of up to 60.8% for hydrogenation of carbon dioxide-rich syngas to aviation kerosene fractions, which is higher than the iron-manganese potassium catalyst (Examples 2, 3, 4) obtained by using citric acid, oxalic acid and urea as organic matter for combustion experiments, and is also higher than the iron-manganese potassium catalyst (Comparative Examples 3, 4) prepared by coprecipitation and impregnation. After further modulating the microwave-assisted heating power in Example 1, it is found that the microwave-assisted heating power is too high or too low, which affects the conversion rate and the selectivity of the aviation kerosene fraction (Examples 5, 6). In addition, the CO conversion rate of the catalyst under the conditions of carbon dioxide-rich syngas atmosphere (Example 1) is higher than the CO conversion rate under the syngas atmosphere (Comparative Example 1), and the CO2 selectivity is also significantly lower. Compared with the traditional heating process (Comparative Example 2), the microwave heating (Example 1) used in the present invention has a higher CO conversion rate and a lower CO2 selectivity, and the selectivity of its aviation kerosene fraction is higher. It can be seen that the catalyst prepared by the method of the present invention has better catalytic performance and higher aviation kerosene fraction selectivity in a carbon dioxide-rich synthesis gas atmosphere.
[0086] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A catalyst for preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas, It is characterized in that The catalyst is a composite metal oxide, which comprises, by mass percentage, 40%-70% Fe, 5%-20% Mn, 5%-20% K and the balance O; When the catalyst is used for the reaction of hydrogenating carbon dioxide-rich synthesis gas to produce aviation kerosene distillate, the CO conversion rate is greater than 55%, and the CO 2 Selectivity <30%, C 8 -C 16 The selectivity to hydrocarbon products is >37%.
2. The method for preparing the catalyst according to claim 1, It is characterized in that The following steps are involved: (1) preparing a precursor solution containing iron, manganese and potassium; (2) adding organic matter to the precursor solution described in step (1) and mixing; (3) The mixed solution in step (2) is subjected to microwave heating and calcination to obtain the catalyst.
3. The method for preparing the catalyst according to claim 2, It is characterized in that In step (1), at least one of the following features is included: (1) The iron source used to prepare the precursor solution includes one or more of iron nitrate, sulfate and chloride; (2) the manganese source used to prepare the precursor solution includes one or more of manganese nitrate, sulfate and chloride; (3) the potassium source used to prepare the precursor solution includes one or more of potassium nitrate, sulfate and chloride; (4) The solvent used to prepare the precursor solution includes water.
4. The method for preparing the catalyst according to claim 2, It is characterized in that In step (1), in the precursor solution, the total concentration of iron, manganese and potassium is 0.1-3.0 mol / L.
5. The method for preparing the catalyst according to claim 2, It is characterized in that In step (2), the organic matter includes one or more of urea, citric acid, oxalic acid, and tartaric acid.
6. The method for preparing the catalyst according to claim 2, It is characterized in that In step (2), the concentration of organic matter in the mixed solution is 0.2-6.0 mol / L.
7. The method for preparing the catalyst according to claim 2, It is characterized in that In step (2), the mixing is performed by stirring in a water bath under heating conditions, the stirring time is 1-4 hours, and the heating temperature is 30-80°C.
8. The method for preparing the catalyst according to claim 2, It is characterized in that In step (3), the power of the microwave heating is 200-800 W, the time is 10-30 min, and the stirring speed is 200-1000 rpm.
9. The method for preparing the catalyst according to claim 2, It is characterized in that In step (3), the calcination temperature is 300-400° C., and the calcination time is 2-6 hours.
10. Use of the catalyst according to claim 1 in preparing aviation kerosene distillate from carbon dioxide-rich synthesis gas, It is characterized in that In the carbon dioxide-rich synthesis gas, CO 2 and (CO+CO 2 ) volume ratio is 1-5:10, H 2 and (CO+CO 2 ) has a volume ratio of 1-3:1; And / or, the reaction temperature for preparing aviation kerosene distillate from the carbon dioxide-rich synthesis gas is 280-360°C, the reaction pressure is 2.0-5.0MPa, and the reaction space velocity is 1000-15000h -1 .
Citation Information
Cited By
Catalyst for preparing sustainable aviation fuel from CO2-rich synthesis gas as well as preparation method and application of catalyst
CN121534781A
Preparation of c5 from a mixed gas + Catalyst for hydrocarbons and method for its preparation and use
CN122912910A