Extraction method of quartz sand

By removing mica by dividing the particle size, combined with magnetic separation, flotation and high-temperature acidification, the problem of difficult to remove fine mica in the prior art is solved, significantly improving the purity and yield of quartz sand, and achieving high-purity quartz Sand extraction.

CN118925929APending Publication Date: 2024-11-12HUNAN LIHUI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411001947.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove finely broken mica from high mica quartz ore, resulting in poor quality of high-purity quartz sand finished products. Especially in venous quartz minerals, it is difficult to completely remove impurities by simply gravity ore dressing, magnetic separation and flotation.

Method used

The method of removing mica by particle size partially, including first crushing screening, magnetic separation, first flotation, secondary crushing screening, calcined water quenching, high-temperature acidification and secondary flotation, through continuous segmented flotation and specific The collector combination gradually removes mica impurities from quartz ore and improves the purity of quartz sand.

Benefits of technology

The thorough removal of fine mica is achieved, the yield and purity of quartz sand is improved, the impurity content is reduced, and the quality of quartz sand is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925929A_ABST
    Figure CN118925929A_ABST
Patent Text Reader

Abstract

The invention provides a quartz sand extraction method which comprises the following steps: firstly, crushing and screening raw ore sample stones for the first time to obtain ore particles with the particle size of 30-50 meshes as a first screened product; then magnetic separation is conducted on the first screening product, most of fine crushed mica sheets with magnetism in ore particles are removed, a magnetic separation product is obtained, and the particle size of the magnetic separation product ranges from 30 meshes to 50 meshes; and primary flotation is conducted on magnetic separation products, under the condition of large particle size, quartz particles are difficult to float out, sand leakage is not prone to occurring, and the effect of improving the yield is achieved. Secondary crushing, grading and screening are conducted on a first flotation product obtained through primary flotation, the particle size of a second screened product is controlled to range from 50 meshes to 160 meshes, and the remaining mica inlaid in the quartz particles can be exposed; the second screened product is subjected to calcination and water quenching and then subjected to high-temperature acidification, other impurities in quartz minerals are removed, then the acidified product is subjected to secondary flotation, a small part of remaining mixed mica sheets are removed, and high-purity quartz sand is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of quartz sand extraction methods, and particularly relates to a quartz sand extraction method. Background Art

[0002] High-purity quartz sand is widely used in high-tech fields such as semiconductors, optical fibers, solar photovoltaics and precision optical instruments due to its high purity, high light transmittance, excellent thermal stability and low thermal expansion coefficient. In the photovoltaic industry, high-purity quartz sand is used in photovoltaic crucibles and reflectors to ensure the purity and efficiency of photovoltaic silicon wafer production, thereby improving the photoelectric conversion efficiency of solar cells and extending their service life. With the popularization of solar power generation, the production of photovoltaic silicon wafers has continued to increase, and the demand for high-purity quartz sand has also increased. Mica, as one of the main impurities of high-purity quartz sand, is the main factor affecting the quality of high-purity quartz sand products. At present, the common mica removal methods mainly include gravity separation, magnetic separation and flotation. Among them, gravity separation uses the difference in mineral density to separate mica from quartz through gravity separation equipment. Gravity separation is only suitable for removing large pieces of mica in pegmatite, and it is difficult to effectively remove fine mica in quartz; magnetic separation mainly uses the difference in mineral magnetism to separate mica from quartz through magnetic separation equipment. Magnetic separation can only remove iron-containing mica, and other iron-free parts such as white mica are difficult to remove; flotation is also a relatively effective method for removing mica, but the selection and use of flotation agents has a great influence on the effect of removing mica, and too much flotation agent is easy to cause sand to escape, resulting in a reduction in the yield; in addition, simple repeated flotation has limited secondary removal effect on mica. At present, a vein quartz mineral has appeared on the market. Due to its good inclusion condition, it is a potential raw material for the preparation of middle and inner crucibles. Its main impurities are fine mica with a particle size of less than 500μm uniformly embedded in the middle of quartz. It is difficult to remove the mica in the mineral by extracting quartz sand from the vein quartz mineral using one or more of the above-mentioned gravity separation method, magnetic separation method and flotation method. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a method for extracting quartz sand, which can extract high-purity quartz sand from high-mica quartz ore.

[0004] A method for extracting quartz sand of the present invention comprises the following steps:

[0005] S100, first crushing and screening: the raw ore sample is first crushed and screened to obtain the first screening product with a particle size of 30-50 mesh;

[0006] S200, magnetic separation: performing magnetic separation on the first screened product to remove magnetic mica to obtain a magnetic separation product;

[0007] S300, first flotation: performing first flotation on the magnetic separation product to obtain a first flotation product;

[0008] S400, secondary crushing and screening: the first flotation product is subjected to secondary crushing and screening to obtain a second screening product of 50 meshes to 160 meshes;

[0009] S500, calcining and water quenching: calcining the second screened product and then performing water quenching to obtain a water quenched product;

[0010] S600, acidification: acidifying the water-quenched product at high temperature to obtain an acidified product;

[0011] S700, secondary flotation: After secondary flotation of the acidified product, it is washed to obtain finished sand;

[0012] S800, drying: drying the finished sand to remove moisture and obtain quartz sand.

[0013] Furthermore, the magnetic field strength of the magnetic separation in step S200 is 1.7-2.1T.

[0014] Furthermore, in step S300, the first flotation adopts continuous segmented flotation, and the first flotation includes a first segment flotation and a second segment flotation; the first segment flotation uses a first collector, coconut amine hydrochloride; the second segment flotation uses a second collector, which is dodecylamine acetate and sodium petroleum sulfonate in a mass ratio of 2:1.

[0015] Furthermore, the dosage of the first collector coconut amine hydrochloride is 700-900 g / t.

[0016] Furthermore, the dosage of the second collector, dodecylamine acetate and sodium petroleum sulfonate, is 750-1000 g / t.

[0017] Furthermore, in step S500, the calcination temperature is 600° C.-900° C., and the calcination time is 10-30 minutes.

[0018] Furthermore, in the step S600, the mass ratio of acid to sand for acidification is 1:1; and the mass ratio of hydrochloric acid to hydrofluoric acid is 3:1.

[0019] Furthermore, in step S700, the secondary flotation adopts continuous segmented flotation, and the secondary flotation includes a third flotation and a fourth flotation; the secondary flotation uses a depressant, sodium hexametaphosphate; the third flotation uses a third collector, which is a mixed hydrochloride of hexadecylamine and octadecylamine in a mass ratio of 1:1; and the fourth flotation uses a fourth collector, which is hexadecyltrimethylammonium bromide.

[0020] Furthermore, the dosage of the third collector hexadecylamine and octadecylamine mixed hydrochloride is 300-500 g / t.

[0021] Furthermore, the fourth collector hexadecyltrimethylammonium bromide is used in an amount of 300-500 g / t.

[0022] The present invention has the following beneficial effects:

[0023] The quartz sand extraction method provided by the present invention adopts the method of partially removing mica by particle size. First, the original ore sample is crushed and screened for the first time to obtain ore particles with a particle size of 30 meshes to 50 meshes as the first screening product; then the first screening product is magnetically separated to remove most of the magnetic fine mica pieces in the ore particles to obtain a magnetic separation product, and the particle size of the magnetic separation product is 30 meshes to 50 meshes; the magnetic separation product with a particle size of 30 meshes to 50 meshes is firstly floated, and in the case of a large particle size, the quartz particles are difficult to be floated out and are not easy to escape sand, thereby achieving the effect of improving the yield of finished products. The first flotation product obtained by the first flotation is subjected to secondary crushing, grading and screening, and the particle size of the second screened product is controlled to be between 50 meshes and 160 meshes, so that the remaining mica embedded in the middle of the quartz particles can be exposed; the second screened product is calcined and water-quenched, and the obtained water-quenched product is subjected to high-temperature acidification to remove other impurities in the quartz mineral to obtain an acidified product, and then the acidified product with other impurities removed is subjected to secondary flotation. The secondary flotation step removes a small part of the mica flakes remaining in the quartz particles, and the product quartz sand has high purity and low impurity content. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of a method for extracting quartz sand provided in some embodiments of the present application. DETAILED DESCRIPTION

[0025] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0026] The present invention provides a method for extracting quartz sand, comprising the following steps:

[0027] S100, first crushing and screening: the raw ore sample is first crushed and screened to obtain the first screening product with a particle size of 30-50 mesh;

[0028] S200, magnetic separation: performing magnetic separation on the first screened product to remove magnetic mica to obtain a magnetic separation product;

[0029] S300, first flotation: performing first flotation on the magnetic separation product to obtain a first flotation product;

[0030] S400, secondary crushing and screening: the first flotation product is subjected to secondary crushing and screening to obtain a second screening product of 50 meshes to 160 meshes;

[0031] S500, calcining and water quenching: calcining the second screened product and then performing water quenching to obtain a water quenched product;

[0032] S600, acidification: acidifying the water-quenched product at high temperature to obtain an acidified product;

[0033] S700, secondary flotation: After secondary flotation of the acidified product, it is washed to obtain finished sand;

[0034] S800, drying: drying the finished sand to remove moisture and obtain quartz sand.

[0035] The quartz sand extraction method disclosed in the present invention adopts the method of partially removing mica according to particle size. First, the original ore sample is crushed and screened for the first time to obtain ore particles with a particle size of 30 meshes to 50 meshes as the first screening product; then the first screening product is magnetically separated to remove most of the magnetic fine mica pieces in the ore particles to obtain a magnetic separation product, and the particle size of the magnetic separation product is 30 meshes to 50 meshes; the magnetic separation product with a particle size of 30 meshes to 50 meshes is firstly floated. In the case of large particle size, quartz particles are difficult to be floated out and sand is not easy to escape, thereby achieving the effect of improving the yield of finished products. The first flotation product obtained by the initial flotation is subjected to secondary crushing, grading and screening, and the particle size of the second screened product is controlled to be between 50 meshes and 160 meshes, so that the remaining mica embedded in the middle of the quartz particles can be exposed; the second screened product is calcined and water-quenched, and the obtained water-quenched product is subjected to high-temperature acidification to remove other impurities in the quartz mineral to obtain an acidified product, and then the acidified product with other impurities removed is subjected to secondary flotation. The secondary flotation step removes a small part of the mica flakes remaining in the quartz particles to obtain a finished sand with a high quartz content, and the finished sand is dried to obtain the target product quartz sand.

[0036] In some embodiments provided by the present invention, the magnetic field strength of the magnetic separation in step S200 is 1.7-2.1 T, and the above magnetic field strength can remove most of the magnetic fine mica flakes.

[0037] In some embodiments provided by the present invention, the first flotation in step S300 adopts continuous segmented flotation, and the first flotation includes a first flotation and a second flotation; the first flotation uses a first collector, coconut amine hydrochloride; the second flotation uses a second collector, which is dodecylamine acetate and sodium petroleum sulfonate in a mass ratio of 2:1. The first flotation adopts continuous segmented flotation. Since different collectors have different adsorption capacities at different sites on the mineral surface, and the combined use of collectors can enhance the adsorption density of the agent on the mineral surface, thereby improving the hydrophobicity of the mineral surface, the present invention uses the first collector, coconut amine hydrochloride, in the first flotation of the first flotation, and uses the second collector, which is dodecylamine acetate and sodium petroleum sulfonate in a mass ratio of 2:1, in the second flotation, to improve the flotation recovery rate. Preferably, the first collector, coconut amine hydrochloride, is used in an amount of 700-900 g / t; the second collectors, dodecylamine acetate and sodium petroleum sulfonate, are used in an amount of 750-1000 g / t; and the increase in the amount of flotation reagents enhances the flotation effect.

[0038] In some embodiments provided by the present invention, the calcination temperature in step S500 is 600°C-900°C, and the calcination time is 10-30 minutes. In this step, the first flotation product is subjected to calcination and water quenching, mainly because the expansion coefficients of the gangue and the target product quartz are quite different, and the calcination and water quenching process allows the two to be selectively dissociated, so that other impurities in the dissociated quartz mineral can be removed by the acidification process in the subsequent step S600.

[0039] In some embodiments provided by the present invention, the acid-sand mass ratio of the acidification in step S600 is 1:1; and the hydrochloric acid and hydrofluoric acid are used in a mass ratio of 3:1. Specifically, the water-quenched product is acidified at a mass ratio of 1:1 with the acid-sand mass ratio being 1:1, and the hydrochloric acid and hydrofluoric acid are used in a mass ratio of 3:1 at 100°C for 12 hours to obtain an acidified product. The mass fraction of the hydrochloric acid used is 37%, and the mass fraction of the hydrofluoric acid is 50%.

[0040] In some embodiments provided by the present invention, the secondary flotation in step S700 adopts continuous segmented flotation, and the secondary flotation includes a third flotation and a fourth flotation; the secondary flotation uses a depressant, sodium hexametaphosphate; the third flotation uses a third collector, which is a mixed hydrochloride of hexadecylamine and octadecylamine in a mass ratio of 1:1; and the fourth flotation uses a fourth collector, which is hexadecyltrimethylammonium bromide. After calcination and water quenching in step S500 and acidification treatment in step S600, the obtained product particles are finer, and the minerals with finer particle size are subjected to secondary flotation. At this time, continuous segmented flotation is still used. Since the particle size of the minerals to be floated at this time is smaller than that of the minerals in the first flotation, the inhibitor sodium hexametaphosphate is added in the secondary flotation process to avoid sand running and increase the recovery rate of the product. At this time, the third stage flotation uses a third collector which is a mixed hydrochloride of hexadecylamine and octadecylamine in a mass ratio of 1:1. The combined collector has higher surface activity than a single collector. The reason is that hexadecylamine is adsorbed on the surface of the gangue, and then the mixed hydrochloride of octadecylamine is adsorbed on the surface of the gangue through the electrostatic attraction with the metal ions on the surface of the gangue and the interaction with the adsorbed hexadecylamine, and a multilayer adsorption film is formed on the surface of the gangue through the electrostatic attraction between the heads of the two and the hydrophobic attraction between the tail chains. Electrostatic force and hydrophobic force can promote the cross adsorption of the two collectors, thereby enhancing the hydrophobicity of the mineral surface; the fourth stage of flotation is to float the mineral by selecting a collector with good adsorption capacity on the mineral surface, and the fourth collector used in the fourth stage of flotation is hexadecyl trimethyl ammonium bromide. Preferably, the inhibitor sodium hexametaphosphate is 100g / t; the third collector hexadecylamine and octadecylamine mixed hydrochloride is used in an amount of 300-500g / t; the fourth collector hexadecyl trimethyl ammonium bromide is used in an amount of 300-500g / t.

[0041] In some implementation modes provided by the present invention, in step S800, the drying temperature of the finished sand is 1000-1200° C., and the drying time is 10-20 minutes.

[0042] The method for extracting quartz sand provided by the present invention is described in detail with specific embodiments below:

[0043] Example 1

[0044] Aiming at a vein quartz mineral with good inclusions on the market, a high-mica quartz ore sample, this embodiment provides a quartz purification method by controlling the different particle size ranges of the mineral for magnetic separation and flotation, which more thoroughly achieves the removal of fine mica, including the following steps:

[0045] S100, first crushing and screening: the high-mica quartz ore sample is first crushed and screened to obtain a product with a particle size of 30-50 mesh;

[0046] S200, magnetic separation: The screened product is subjected to magnetic separation with a magnetic field strength of 1.7-2.1T to remove some magnetic mica;

[0047] S300, first flotation: including the first flotation and the second flotation; in the first flotation, the pH value is adjusted to 3-5 with sulfuric acid, the temperature is 50°C, and the first collector coconut amine hydrochloride 700g / t is used. After flotation for 20-30 minutes, water is changed for washing; in the second flotation, the pH value is adjusted to 3-5 with hydrofluoric acid, the temperature is 50°C, and the second collector is dodecylamine acetate and sodium petroleum sulfonate 800g / t in a mass ratio of 2:1. After flotation for 20-30 minutes, water is changed for washing to obtain the first flotation product;

[0048] S400, secondary crushing and screening: the first flotation product is subjected to secondary crushing and screening to obtain a second screening product of 50 meshes to 160 meshes;

[0049] S500, calcination and water quenching: calcining the second screened product at a temperature range of 600° C. to 900° C. for 10 to 30 minutes, performing water quenching treatment, and obtaining a water quenched product;

[0050] S600, acidification: Use hydrochloric acid and hydrofluoric acid in a mass ratio of 3:1, and acidify the water-quenched product at a mass ratio of acid to sand of 1:1, and acidify at high temperature at 100°C for 12 hours; wherein the mass fraction of hydrochloric acid is 37%, and the mass fraction of hydrofluoric acid is 50%;

[0051] S700, secondary flotation: including the third and fourth flotation stages; in the first flotation stage, the pH value is adjusted to 3-5 with hydrofluoric acid, the temperature is 50°C, 100g / t of sodium hexametaphosphate inhibitor is added first, and then 300g / t of mixed hydrochloride of hexadecylamine and octadecylamine with a mass ratio of 1:1 as the third collector is used, and the third flotation stage is carried out for 20-30 minutes, and the water is changed for rinsing; the pH value is adjusted to about 4 with hydrofluoric acid again, and 450g / t of hexadecyltrimethylammonium bromide as the fourth collector is added, and the flotation is carried out for 20-30 minutes, and the water is changed for rinsing. The obtained flotation product is washed twice with ethanol and three times with deionized water to obtain the finished sand;

[0052] S800, drying: passing the finished sand through a high-purity quartz tube at 1100°C for 10 minutes to dry out the moisture and obtain quartz sand.

[0053] Comparative Example 1

[0054] The comparative example is to extract quartz sand from a high-mica quartz ore sample using a conventional flotation process, and the method comprises the following steps:

[0055] S100, crushing: crush and screen the high mica sample to obtain products with a particle size of 50-180 mesh;

[0056] S200, calcination and water quenching: calcining the product obtained in the previous step at a temperature range of 600°C-900°C for 10min-30min, and water quenching;

[0057] S300, flotation: adjust the pH value to 3-5 with hydrofluoric acid, temperature 50°C, collector is 2:1 dodecylamine acetate and sodium petroleum sulfonate 800g / t, flotation for 20-30 minutes, change water for washing;

[0058] S400, acidification: Use hydrochloric acid and hydrofluoric acid in a mass ratio of 3:1, and the acid-sand mass ratio is 1:1, and acidify at 100°C for 12 hours. The mass fraction of hydrochloric acid is 37%, and the mass fraction of hydrofluoric acid is 50%;

[0059] S500, flotation: adjust the pH value to 3-5 with hydrofluoric acid, temperature to 50°C, first add 100g / t of sodium hexametaphosphate inhibitor, 300g / t of mixed hydrochloride of hexadecylamine and octadecylamine in a mass ratio of 1:1, float until the foam is gone, and rinse with water;

[0060] S600, drying: passing the product obtained in the previous step through a high-purity quartz tube at 1100° C. for 10 minutes to dry out the water and obtain a conventional flotation product.

[0061] The products obtained in Example 1 and Comparative Example 1 were subjected to elemental analysis, and the elemental impurity contents thereof are shown in Table 1, in units of ppm.

[0062] Table 1

[0063]

[0064]

[0065] The mica in the vein quartz mineral used in Example 1 and Comparative Example 1 is an iron mica, and its chemical formula is KFe3(AlSi3O 10 )(OH)2. As shown in Table 1, the contents of the three elements of iron, aluminum and potassium in the quartz sand obtained in Example 1 are much lower than those in Comparative Example 1. The contents of the three elements of iron, aluminum and potassium reflect the contents of mica impurities in the quartz sand. From this result, it can be seen that Example 1 using the method of the present invention has a better effect on removing mica. In addition, the sodium content in Comparative Example 1 is 3.47ppm, while the sodium content in Example 1 is only 1.12ppm. The sodium content can be used to characterize the content of feldspar. It can be inferred that the method of the present invention is more effective than conventional methods in removing trace feldspar in vein quartz minerals.

[0066] The above-mentioned difference in flotation effect is due to the fact that when the conventional process is adopted, the crushing step crushes the quartz particles into finer particle sizes. During the first flotation, the reagent has already attached to the active sites, resulting in the flotation reagent being unable to contact the active sites of the impurity components during the subsequent second flotation, resulting in poor flotation effect. At the same time, it causes excess flotation reagent in the system, which can easily cause sand leakage and affect the recovery rate.

[0067] The above is a detailed introduction to a method for extracting quartz sand provided by the present invention. This article uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the core idea of ​​the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for extracting quartz sand, characterized in that: The following steps are involved: S100, first crushing and screening: the raw ore sample is first crushed and screened to obtain the first screening product with a particle size of 30-50 mesh; S200, magnetic separation: performing magnetic separation on the first screened product to remove magnetic mica to obtain a magnetic separation product; S300, first flotation: performing first flotation on the magnetic separation product to obtain a first flotation product; S400, secondary crushing and screening: the first flotation product is subjected to secondary crushing and screening to obtain a second screening product of 50-160 mesh; S500, calcining and water quenching: calcining the second screened product and then performing water quenching to obtain a water quenched product; S600, acidification: acidifying the water-quenched product at high temperature to obtain an acidified product; S700, secondary flotation: After secondary flotation of the acidified product, it is washed to obtain finished sand; S800, drying: drying the finished sand to remove moisture and obtain quartz sand.

2. The method for extracting quartz sand according to claim 1, characterized in that: The magnetic field strength of the magnetic separation in step S200 is 1.7-2.1T.

3. The method for extracting quartz sand according to claim 1, characterized in that: In step S300, the first flotation adopts continuous segmented flotation, and the first flotation includes a first segment flotation and a second segment flotation; The first stage flotation uses a first collector, coconut amine hydrochloride; the second stage flotation uses a second collector, which is dodecylamine acetate and sodium petroleum sulfonate in a mass ratio of 2:

1.

4. The method for extracting quartz sand according to claim 3, characterized in that: The first collector coconut amine hydrochloride is used in an amount of 700-900 g / t.

5. The method for extracting quartz sand according to claim 3, characterized in that: The dosage of the second collector, dodecylamine acetate and sodium petroleum sulfonate, is 750-1000 g / t.

6. The method for extracting quartz sand according to claim 1, characterized in that: In the step S500, the calcination temperature is 600° C.-900° C., and the calcination time is 10-30 minutes.

7. The method for extracting quartz sand according to claim 1, characterized in that: The mass ratio of acid to sand in the acidification in step S600 is 1:1; the mass ratio of hydrochloric acid to hydrofluoric acid is 3:

1.

8. The method for extracting quartz sand according to claim 1, characterized in that: In step S700, the secondary flotation adopts continuous segmented flotation, and the secondary flotation includes a third flotation and a fourth flotation; the secondary flotation uses sodium hexametaphosphate as an inhibitor; the third flotation uses a third collector which is a mixed hydrochloride of hexadecylamine and octadecylamine in a mass ratio of 1:1; and the fourth flotation uses a fourth collector which is hexadecyltrimethylammonium bromide.

9. The method for extracting quartz sand according to claim 8, characterized in that: The dosage of the third collector hexadecylamine and octadecylamine mixed hydrochloride is 300-500 g / t.

10. The method for extracting quartz sand according to claim 8, characterized in that: The fourth collector hexadecyltrimethylammonium bromide is used in an amount of 300-500 g / t.

Citation Information

Cited By

  • Method for separating and purifying high-purity quartz sand from series of rocks of twinkling, quartz twinkling, granite twinkling and granite

    CN120205309A

  • A method for separating and purifying high-purity quartz sand from diorite, quartz diorite, granodiorite and granite series rocks