Microtexture regeneration cooling flow channel and preparation method and application thereof

By forming rectangular microgrooves on the inner wall of the cooling channel in the combustion chamber of aerospace engines and then performing acid washing, the problems of poor cooling effect and high cost of existing cooling channel structures have been solved, achieving more efficient cooling and lower manufacturing costs.

CN118926532AActive Publication Date: 2024-11-12ARMOR ACADEMY OF CHINESE PEOPLES LIBERATION ARMY

Patent Information

Application Number
CN202410990787.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing cooling channel structure of aerospace engine combustion chamber has problems such as low contact rate between coolant and inner wall, poor structural rigidity, high development cost, high risk of coking, poor space utilization and high thermal conductivity, resulting in poor cooling effect.

Method used

A selective laser melting additive manufacturing method was used to integrally form a flow-oriented rectangular microgroove on the inner wall of the regenerated cooling channel, and the microtextured regenerated cooling channel was prepared by acid washing under ultrasonic conditions with a mixed acid solution of hydrofluoric acid and nitric acid.

Benefits of technology

It significantly improves the coolant flow rate and the heat transfer coefficient between the wall and the coolant, reduces the inner wall temperature, enhances the cooling effect, and reduces manufacturing costs. It has wide applicability and good compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926532A_ABST
    Figure CN118926532A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of regenerative cooling, and particularly relates to a micro-texture regenerative cooling flow channel and a preparation method and application thereof. According to the method, a selective laser melting additive manufacturing method is adopted to integrally generate a forward rectangular micro groove in the inner wall face of a regeneration cooling channel, then a mixed acid solution is adopted for acid pickling under the ultrasonic condition, the micro-texture regeneration cooling channel is obtained, and the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid. The micro-texture regenerative cooling flow channel is integrally machined and formed through SLM, accurate control over the shape of the cross section of the machined rectangular micro-groove is achieved, and the obtained micro-texture regenerative cooling flow channel is uniform in flow under the condition that the total coolant flow is not changed. The coolant flow in the cooling channel of the regenerative cooling combustion chamber and the uniformity of the same section temperature can be improved, so that local damage to the combustion chamber caused by overheating gasification of the coolant at a certain position is prevented, and uniform and effective cooling of the regenerative cooling combustion chamber is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of regenerative cooling, and in particular relates to a micro-textured regenerative cooling channel and a preparation method and application thereof. Background Art

[0002] Space engines have been a hot research and development issue in the aerospace field in recent years. Space engines refer to engines that use liquid fuel and oxidizer as energy sources. They are composed of combustion chambers, propellant supply systems, and engine control systems. The combustion chamber is a component that converts the chemical energy of the propellant into jet kinetic energy; the nozzle expands and accelerates the high-temperature combustion gas to produce a high-speed jet. When the space engine is working, the extremely high aerodynamic and thermal loads brought by the ultra-high flight Mach number and the extremely high temperature generated by the combustion of hydrocarbon fuel propellants exceed the bearing capacity of existing materials. In view of this problem, one of the keys to designing a space engine is to solve the thermal protection problem of the aircraft, especially the cooling problem of the combustion chamber of the space engine. The existing coolant is used to cool the thrust chamber, and the liquid fuel used by the engine itself is usually used as the cooling medium. The liquid fuel flows in the opposite direction to the external high-temperature gas in the cooling channel inside the wall of the high-temperature component, absorbs heat through forced convection heat exchange, and thus reduces the wall temperature. When the liquid fuel leaves the high-temperature component, on the one hand, the high-temperature component is cooled, and on the other hand, the liquid fuel enters the combustion chamber at a higher temperature, realizing energy regeneration. Therefore, this convection cooling method is called regenerative cooling.

[0003] The cooling channel structures widely used in modern engine combustion chambers are divided into: corrugated plate cooling channel, milling slot cooling channel and tube bundle cooling channel. Among them, due to its structural characteristics, half of the coolant in the corrugated plate cooling channel cannot directly contact the inner wall, which is not conducive to reducing the temperature of the inner wall; although the tube bundle cooling channel has a light structure and fast heat dissipation, it is mostly used for large-area, low heat flux, and high-speed nozzle extensions; the inner wall milling slot type is to mill out cooling slots on the inner wall surface, and connect the outer wall surface with the inner wall surface by welding to form a cooling channel. Traditional cooling channel manufacturing methods, such as corrugated plate structures, have the disadvantages of low contact rate between coolant and actual interface, resulting in low heat exchange efficiency; the tube bundle structure is limited by poor structural rigidity and high development cost; the milling slot structure, on the one hand, due to the risk of fuel coking, the flow channel in the traditional regenerative cooling structure should not be too flat, and the space utilization rate in the wall thickness direction is poor, and there is still a lot of room for weight reduction; on the other hand, metal materials with large thermal conductivity in the thickness direction account for a large proportion, resulting in a small equivalent thermal resistance in this direction, and the thermal insulation capacity needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to provide a micro-textured regenerative cooling channel and a preparation method and application thereof. The micro-textured regenerative cooling channel provided by the present invention can significantly improve the product quality of the micro-groove structure on the inner wall of the regenerative cooling pipeline, improve the processing accuracy and reduce the manufacturing cost. The obtained micro-groove structure can increase the flow rate of the coolant in the regenerative cooling channel, increase the heat exchange coefficient between the wall and the coolant, effectively reduce the inner wall temperature, and have a better cooling effect.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a micro-textured regenerative cooling channel, comprising the following steps:

[0007] A selective laser melting additive manufacturing method is used to form a downstream rectangular micro-groove on the inner wall of the regenerative cooling channel, thereby obtaining an initial micro-groove structure on the inner wall of the regenerative cooling channel;

[0008] The initial micro-groove structure is pickled with a mixed acid solution under ultrasonic conditions to obtain the micro-texture regeneration cooling channel, and the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid.

[0009] Preferably, the cross-section of the downstream rectangular micro-grooves is rectangular, the groove width and groove depth of the grooves are independently 200-500 μm; and the groove spacing is 400-1000 μm.

[0010] Preferably, the particle size of the molding powder used in the selective laser melting is 15 to 53 μm; the molding powder used in the selective laser melting is TA15 titanium alloy powder.

[0011] Preferably, the selective laser melting is performed by placing the regenerative cooling channel horizontally and processing vertically;

[0012] The conditions for the selective laser melting include: the laser type is a continuous laser, the scanning path is a zigzag path, the thickness of the powder layer is 0.02-0.08 mm, the diameter of the laser spot is 80 μm, and the processing angle is 90°.

[0013] Preferably, the power of the continuous laser is 150-300 W, the scanning speed is 800-1400 mm / s, and the scanning interval is 0.06-0.16 mm.

[0014] Preferably, the mixed acid solution of hydrofluoric acid and nitric acid comprises HF, HNO 3 and water; in the mixed acid solution of hydrofluoric acid and nitric acid: the mass percentage of HF is 1 to 10%, the HNO 3 The mass percentage is 10-20%.

[0015] Preferably, the ultrasonic conditions include: the ultrasonic power is 400-500W, the frequency is 40-60kHz; the pickling temperature is 20-60°C, and the time is 3-5min.

[0016] Preferably, after obtaining the initial micro-groove structure and before performing the pickling, the method further comprises: flushing the initial micro-groove structure, wherein the flushing is performed using high-pressure gas, and the pressure of the high-pressure gas is 0.3-0.6 MPa.

[0017] The present invention provides a micro-textured regenerative cooling channel prepared by the preparation method described in the above technical solution, wherein the inner wall surface of the micro-textured regenerative cooling channel has an integrated downstream rectangular micro-groove.

[0018] The present invention provides application of the micro-textured regenerative cooling flow channel described in the above technical solution in thermal protection of an engine combustion chamber.

[0019] The present invention provides a method for preparing a micro-textured regenerative cooling channel, comprising the following steps: using an additive manufacturing method of selective laser melting (SLM) to form a downstream rectangular micro-groove on the inner wall of the regenerative cooling channel, and obtaining an initial micro-groove structure on the inner wall of the regenerative cooling channel; using a mixed acid solution to pickle the initial micro-groove structure under ultrasonic conditions to obtain the micro-textured regenerative cooling channel, wherein the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid. The present invention forms a micro-texture in the regenerative cooling channel through SLM integrated processing, thereby achieving precise control of the cross-sectional shape of the processed micro-groove, including the contour, micro-texture width, and micro-texture depth; and processing the inner wall of the raw cooling pipe to obtain a surface feature with a precisely controllable cross-sectional shape and a smooth bottom morphology. Compared with the traditional method of microfluidic channel processing microtexture (such as laser etching process, mainly to achieve microtexture processing in the Z-axis direction), the microtexture of the microtexture regenerative cooling channel obtained by SLM integrated processing in the present invention can achieve microtexture arrangement in the X and Y-axis directions, breaking the limitations of traditional methods. The preparation method of the microtexture regenerative cooling channel provided by the present invention can significantly improve product quality, improve processing accuracy and reduce manufacturing costs. The microtexture of the microfluidic channel processed by the present invention can increase the flow rate of the coolant, increase the heat exchange coefficient between the wall and the coolant, and effectively reduce the temperature of the inner wall, which has a better cooling effect than the existing structure. The experimental results of the embodiment show that the microtexture regenerative cooling channel obtained by SLM integrated processing in the present invention reduces the average velocity at the boundary due to the presence of microgrooves, and the thickness of the velocity boundary layer is thinned, which destroys the flow structure of the original boundary layer, making the momentum and energy exchange between the fluids at the boundary more intense, and confirming the flow resistance regulation and enhanced heat exchange effect of the microgrooves. The micro-textured regenerative cooling flow channel prepared by the present invention can improve the coolant flow rate in the cooling channel of the regenerative cooling combustion chamber and the uniformity of the temperature of the same cross section under the condition that the total coolant flow rate remains unchanged, thereby preventing the coolant from being overheated and gasified somewhere, causing local damage to the combustion chamber, and ensuring uniform and effective cooling of the regenerative cooling combustion chamber. The present invention can be quickly adapted according to the actual engine structure, has the advantages of wide applicability, economy, convenience and significant effect, and solves the problems of the prior art in terms of unclear drag reduction effect and poor adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A zigzag scanning path diagram in an embodiment of the present invention;

[0021] Figure 2 The microscopic morphology of different areas on the surface of sample No. 10 in Example 1 of the present invention is as follows: Figure 2 (a) is the morphology of area A. Figure 2 (b) in the figure shows the morphology of area B. Figure 2(c) in the figure is the morphology of the C region. Figure 2 (d) in the figure is the morphology of region D. Figure 2 (e) in the figure shows the morphology of region E;

[0022] Figure 3 The microscopic morphology of the B area of ​​the 4th, 7th, 10th and 13th samples in Example 1 of the present invention is as follows: Figure 3 (a) is sample No. 4, Figure 3 (b) is sample No. 7. Figure 3 (c) in the figure is sample No. 10. Figure 3 (d) in the figure is sample No. 13;

[0023] Figure 4 The microscopic morphology of the B area of ​​the 10th, 12th and 11th samples in Example 1 of the present invention is as follows: Figure 4 (a) is sample No. 10, Figure 4 (b) is sample No. 12. Figure 4 (c) in the figure is sample No. 11;

[0024] Figure 5 This is a specific implementation diagram of pickling during pickling in an embodiment of the present invention;

[0025] Figure 6 The surface morphology of 200μm micro-groove structure under different pickling time;

[0026] Figure 7 This is an EDS layered image of a sample that has not been pickled in an embodiment of the present invention;

[0027] Figure 8 This is an EDS layered image of the sample after pickling with the pickling solution 6 nitric acid + nitric acid double acid in the embodiment of the present invention;

[0028] Fig. 9 A circulating water tunnel platform used in the embodiment of the present invention;

[0029] Fig. 9 Middle: 1-test section, 2-water tank, 3-insulation layer, 4-heating plate, 5-wall to be heated, 6-thermocouple, 7-temperature transmitter, 8-wall to be insulated, 9-pressure differential transmitter, 10-electromagnetic flowmeter, 11-centrifugal pump, 12-motor inverter, 13-inlet contraction section; 14-outlet expansion section;

[0030] Fig.10 This is a temperature variation diagram of the heat insulation wall surface of the regenerative cooling flow channel in an embodiment of the present invention;

[0031] Fig.11 Schematic diagram of micro-groove structure;

[0032] Fig.12 is the process parameter sample model;

[0033] Fig.13 It is the actual effect diagram of the SLM forming process parameter sample in the embodiment;

[0034] Fig.14 Surface morphology of the samples after pickling with different pickling solutions: Fig.14 (a) is pickling solution 1, Fig.14 (b) is pickling solution 2, Fig.14 (c) in the above is pickling solution 3, Fig.14 (d) in the above is pickling solution 4, Fig.14 (e) is pickling solution 5;

[0035] Fig.15 The micro-groove structure morphology: Fig.15 (a) is a cooling channel with a micro-groove structure. Fig.15 (b) shows the optimized 200 μm micro-groove three-dimensional morphology. Fig.15 (c) in the figure is the cross-sectional profile curve after optimization. DETAILED DESCRIPTION

[0036] The present invention provides a method for preparing a micro-textured regenerative cooling channel, comprising the following steps:

[0037] A selective laser melting additive manufacturing method is used to form a downstream rectangular micro-groove on the inner wall of the regenerative cooling channel, thereby obtaining an initial micro-groove structure on the inner wall of the regenerative cooling channel;

[0038] The initial micro-groove structure is pickled with a mixed acid solution under ultrasonic conditions to obtain the micro-texture regeneration cooling channel, and the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid.

[0039] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0040] Although SLM metal additive manufacturing technology has very good application prospects in the field of aerospace, due to the inherent step effect, spheroidization effect, powder adhesion and other characteristics in its additive manufacturing process, the surface quality of current commercial SLM molded parts is generally poor and the surface roughness is high. For the regenerative cooling channel of the aerospace engine, the inner surface of the cooling channel has the function of efficiently transferring the cooling medium. The inner surface morphology of the channel has a significant impact on the flow state and heat exchange efficiency of the cooling medium in the cooling channel, which will seriously affect the use characteristics of the regenerative cooling channel. The present invention achieves precise control of the SLM forming quality, reduces surface roughness, and improves the accuracy and consistency of the micro-groove design and the actual forming contour.

[0041] The present invention adopts a selective laser melting additive manufacturing method to form a downstream rectangular micro groove on the inner wall of the regenerative cooling channel, and obtains an initial micro groove structure on the inner wall of the regenerative cooling channel. The present invention selects groove texture as the rough element of the inner wall of the flow channel. On the one hand, the groove texture is relatively simple, with few variables and easy to control; on the other hand, the groove texture has a relatively complete drag reduction and heat exchange enhancement mechanism. In the present invention, the particle size of the molding powder used in the selective laser melting is preferably 15 to 53 μm. In a specific embodiment of the present invention, the molding powder used in the selective laser melting is preferably TA15 titanium alloy powder. TA15 titanium alloy powder is spherical. In a specific embodiment of the present invention, the mass percentage of Al element in the TA15 titanium alloy powder is 5.5%, the mass percentage of Zr element is 1.5%, and the mass percentage of Mo element is 0.5%. The mass percentage of V element is 0.8%, and the balance is Ti element.

[0042] In a specific embodiment of the present invention, the additive manufacturing equipment used in the selective laser melting is the M290 metal 3D printer produced by the German EOS company. The equipment can realize the sintering of metal powder by laser beam in layer units. The equipment adopts the method of downward powder feeding and one-way powder spreading. The protective gas of the equipment is compatible with argon (Ar) and nitrogen (N 2 ) are used to reduce the oxygen content in the chamber to less than 0.02% to prevent the workpiece from oxidizing; and the equipment has the advantage of being able to directly use CAD data to quickly, flexibly and economically produce metal parts.

[0043] In the present invention, the present invention integrally forms "rectangular micro grooves in the downstream direction". Compared with the transverse micro grooves, the longitudinal micro grooves have good enhanced heat exchange performance and will not significantly increase the flow resistance in the flow channel. At the same time, the present invention considers the influence of the step effect in the SLM forming process, abandons the triangular grooves, and selects the rectangular grooves with higher forming quality as the modified texture of the inner wall of the flow channel. The micro groove morphology in the present invention is as follows Fig.11 As shown in Figure 2, p, s, and h represent the micro-groove spacing, groove width, and groove depth, respectively, and α = 90°.

[0044] In a specific embodiment of the present invention, the groove width and groove depth of the micro groove are preferably equal, and the groove width s=groove depth h is preferably 200-500 μm, and is particularly preferably 200 μm, 300 μm, 400 μm or 500 μm. The groove pitch p is preferably 400-1000 μm, and is particularly preferably 400 μm, 600 μm, 800 μm or 1000 μm.

[0045] In the present invention, the selective laser melting is preferably carried out by horizontal placement of the regenerative cooling channel and vertical processing. The conditions for the selective laser melting preferably include: the laser type is preferably a continuous laser, the scanning path is preferably a zigzag path, and the thickness of the powder layer is preferably 0.02-0.08 mm, specifically preferably 0.03 mm. The diameter of the laser spot is preferably 80 μm, and the processing angle is preferably 90°. The power of the continuous laser is preferably 150-300 W, more preferably 150 W, 200 W, 250 W, 275 W or 300 W, and the gradient of the power change of the continuous laser is preferably 50 W. The scanning speed is preferably 800-1400 mm / s, more preferably 800 mm / s, 1000 mm / s, 1200 mm / s, 1250 mm / s or 1400 mm / s. The scanning spacing is preferably 0.06 to 0.16 mm, more preferably 0.06 to 0.12 mm, specifically preferably 0.1 mm, 0.12 mm, 0.14 mm or 0.16 mm, and the variation gradient of the scanning spacing is preferably 20 μm.

[0046] In the present invention, the laser volume energy density of the continuous laser is as shown in Formula 1:

[0047] Ev=P L / (V S ×H S ×D S ) Formula 1,

[0048] In formula 1: P L is the power of continuous laser, V S is the scanning speed, H S is the scanning distance, D S To lay a thick layer of powder.

[0049] After the initial micro-groove structure is obtained on the inner wall of the regeneration cooling channel, the present invention uses a mixed acid solution to pickle the initial micro-groove structure under ultrasonic conditions to obtain microchannels on the inner wall of the regeneration cooling channel, and the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid.

[0050] In the present invention, after obtaining the initial micro-groove structure and before performing the pickling, the present invention preferably further comprises: flushing the initial micro-groove structure, the flushing is performed using high-pressure gas, and the pressure of the high-pressure gas is preferably 0.3-0.6MPa. The present invention preferably uses high-pressure gas to perform preliminary flushing on the SLM formed metal parts (containing the initial micro-groove structure) to remove metal powder and dust on the surface of the SLM formed metal parts. After the flushing, a flushed sample is obtained, and the present invention preferably further comprises: using a steel brush to preliminarily clean the loose powder and dust on the surface of the initial micro-groove structure of the flushed sample.

[0051] In the present invention, the role of pickling is to remove powder sticking to the surface of the sample and prevent excessive corrosion of microtexture.

[0052] In the present invention, the mixed acid solution of hydrofluoric acid and nitric acid preferably comprises HF, HNO 3 and water. The water is preferably deionized water. In the mixed acid solution of hydrofluoric acid and nitric acid: the mass percentage of HF is preferably 1-10%, specifically preferably 1%, 3%, 5% or 10%, and most preferably 3%, and the HNO 3 The mass percentage of is preferably 10-20%, and specifically preferably 20%.

[0053] In the present invention, the ultrasonic conditions include: the ultrasonic power is preferably 400-500W, and the frequency is preferably 40-60kHz. The pickling is preferably: immersing the sample containing the initial micro-groove structure in a mixed acid solution for pickling. The pickling temperature is preferably 35°C. The pickling time is preferably 3-5min. The pickling is preferably carried out under the condition of water bath heating.

[0054] In the present invention, the pickling time of the pickling should not be too short, otherwise the pickling will not be thorough, and powder will remain on the surface of the micro-texture, affecting the drag reduction effect; at the same time, with the extension of the pickling time, the pickling solution will cause serious corrosion to the micro-texture structure while removing sticky powder and surface micro-burrs. However, in the present invention, "double acid solution" is used for pickling (i.e. double acid pickling). Due to the addition of nitric acid, a layer of oxide film is formed on the surface of the sample during double acid pickling, thereby effectively protecting the main body of the texture and preventing damage to the texture while removing the surface micro-burrs.

[0055] In the present invention, after the pickling, the present invention preferably dries the obtained pickling sample to obtain the micro-textured regeneration cooling channel. In the present invention, the drying is preferably oven drying.

[0056] The present invention provides a micro-textured regenerative cooling channel prepared by the preparation method described in the above technical solution, wherein the inner wall surface of the micro-textured regenerative cooling channel has an integrated downstream rectangular micro-groove.

[0057] The present invention provides application of the micro-textured regenerative cooling flow channel described in the above technical solution in thermal protection of an engine combustion chamber.

[0058] In the present invention, the engine combustion chamber is specifically an aerospace engine combustion chamber.

[0059] In summary, the technical effects of the present invention are:

[0060] 1. Compared with other micro-texturing processing technologies, the laser surface micro-texturing processing technology used in the present invention can be carried out in an atmospheric environment without pollution to the environment, is simple to manufacture and does not require other process assistance, has low equipment cost, a wide range of processing objects, and can control appropriate size and morphology. Therefore, the selective laser melting (SLM) technology is considered to be one of the most promising processing technologies in the field of drag reduction surface micro-texturing processing. It has the processing advantages of wide material adaptability, minimal heat-affected zone, and almost no recasting.

[0061] 2. The present invention adopts ultrasonic assisted pickling. The bubbles generated by the high-frequency ultrasonic waves will grow at the connection between the particles and the surface. Under the repeated impact of the bubbles, the unmelted particles on the surface of the sample can be completely removed; thereby, most of the unmelted particles on the SLM surface and the powder adsorbed on the surface of the sample can be effectively removed, and the pickling process can be further accelerated. At the same time, the uniformity of the pickling is better, and the pitting problem caused by local excessive pickling is effectively reduced.

[0062] 3. The present invention adopts double acid for pickling. Compared with single acid pickling, the single acid pickling reaction is more intense than double acid pickling, the time required for pickling is also less, and heating helps to improve the surface quality of pickling and greatly shorten the time required for pickling (too high pickling temperature will cause the acid solution to volatilize and affect the concentration, and the volatilized acid vapor is harmful to the human body, so this experiment uses a heating temperature of 35°C).

[0063] 4. The method provided by the present invention is simple to operate and has low requirements on equipment. At the same time, it effectively meets the heat exchange requirements of the combustion chamber wall and ensures the reliability of the regenerative cooling channel layout scheme. This method is flexible. It can shorten the product processing cycle and cost, effectively reduce product defects, and meet the actual application requirements of aerospace combustion chambers.

[0064] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0065] Example 1

[0066] This embodiment provides a method for manufacturing micro-texture of the inner wall of a cooling channel based on SLM integrated processing of micro-texture regeneration, comprising the following steps:

[0067] In the embodiment, a rectangular groove texture is selected as the rough element of the inner wall of the flow channel. On the one hand, the groove texture is relatively simple, with few variables and easy to control; on the other hand, the groove texture has a relatively complete mechanism for reducing drag and enhancing heat exchange.

[0068] In this embodiment, in order to more efficiently explore the influence of different process parameters on the forming quality of micro grooves of different scales, four surface structures are designed on a rectangular parallelepiped model with a geometric size of 50 mm × 10 mm and a height of 2 mm, namely, a smooth wall, a micro groove wall with s = h = 200, 300, 400, and 500 μm, as shown in FIG. Fig.12 The microgroove dimensions of different regions are shown in Table 1.

[0069] Table 1 Microgroove dimensions in different areas

[0070]

[0071] In this embodiment, the same sample is prepared using the same process parameters, and the number of samples is determined according to the set parameter range. To ensure the quality of micro-groove formation, all samples are printed vertically in the same direction as the micro-grooves, and the samples are arranged sparsely and staggered to avoid mutual interference between the samples.

[0072] In this embodiment, the metal 3D printer used has a SLM powder particle size of 15 to 53 microns, a continuous laser, and a zigzag scanning path (such as Figure 1 The fixed parameters are as follows: the powder thickness is 0.03mm, the spot size is 0.08mm, and the processing angle is 90° horizontal placement and vertical processing. The orthogonal variables are laser power (150-300W), scanning speed (800-1400mm / s) and scanning spacing (0.06-0.12mm). A three-factor four-level orthogonal experiment is designed. The orthogonal experiment is shown in Table 2.

[0073] Table 2 SLM process parameters orthogonal experiment parameter settings

[0074]

[0075] Fig.13 This is the actual effect diagram of the SLM forming process parameter sample in this embodiment. Fig.13 It can be seen that the 16 sets of process parameter combinations selected can completely print the designed sample structure and micro-groove structures of different scales at the macro level, indicating that the process parameter range obtained in the preliminary experiment is relatively reasonable. In order to further analyze the influence of process parameters on the micro-groove forming quality and find the optimal process parameters, a large number of invalid parameter combinations were eliminated.

[0076] Figure 2 The microscopic morphology of different areas on the surface of sample No. 10: Figure 2 (a) is the morphology of area A. Figure 2 (b) in the figure shows the morphology of area B. Figure 2 (c) in the figure is the morphology of the C region. Figure 2 (d) in the figure is the morphology of region D. Figure 2 (e) in the figure shows the morphology of zone E.

[0077] from Figure 2 It can be seen that under the same process parameters, compared with the smooth surface Figure 2 (a) SLM additive manufacturing, the micro-groove structure surface is as follows Figure 2 The powder sticking in (b), (c), (d), and (e) is greatly improved, and the forming quality is much worse. This is because the micro-groove structure has more detailed sizes, and the laser scanning process requires frequent starts and stops. The forming quality at the beginning and end of the molten pool is compared with continuous scanning, which will make it difficult to ensure the quality of the formed micro-groove structure. On the other hand, due to the limitation of the laser spot diameter, the resolution is insufficient when preparing fine structures. At the same time, the micro-groove structure itself is prone to gas reflux at the bottom of the groove, which is also more likely to cause powder sticking and powder accumulation. However, as the size of the micro-groove increases, the above problems will be greatly improved, which means that the process parameters that can achieve high-quality preparation of small-scale micro-groove structures often have better forming quality when preparing large-scale micro-groove structures.

[0078] Figure 3 The microscopic morphology of 200μm micro-groove under different laser power and scanning speed combination process parameters when the scanning spacing is 0.16mm. Figure 3 As can be seen from (a) and (b) in the figure, when the laser power and scanning speed are low, the laser volume energy density input is insufficient, causing a large amount of metal powder to enter the molten pool before it is completely melted. As the molten pool cools, this part of the powder also solidifies in it, resulting in a significant increase in the roughness of the molten pool after solidification. As the error accumulates, the continuity and integrity of the formed micro-groove structure are poor. Sample No. 10 Figure 3 (c) in the figure increases the scanning speed while increasing the laser power compared to samples 4 and 7, and the final micro-groove forming quality is significantly improved. This is because if the laser power is simply increased, the laser spot focusing time will be too long, the energy input per unit time of the molten pool will be too large, the molten pool will become extremely unstable, the spheroidization effect will become more obvious, and the splashing molten droplets will cause the micro-groove surface quality to deteriorate. However, this does not mean that higher laser power and faster scanning speed will lead to better micro-groove forming quality. Sample 13, for example, Figure 3 The surface quality of (d) in the figure is worse than that of sample No. 10. This is because higher laser power means that the instantaneous energy input is too large and the molten pool is active, but the excessive scanning speed will cause the molten pool to cool rapidly. It is in this rapid energy input and rapid energy withdrawal that the metal powder becomes more active, and the micro-groove forming quality will decrease instead of increase. Therefore, it is necessary to match the laser power and scanning speed to obtain a high-quality micro-groove structure.

[0079] Figure 4The microscopic morphologies of the micro grooves at different scanning intervals are shown in Figure 2. Figure 4 As can be seen in (a), due to the large scanning interval used in sample No. 10, the liquid metal in the remelting expansion zone is insufficient to fully replenish this area, resulting in a depression in the remelting expansion zone in the two scanning paths, which makes it easy for inclusions to occur here and the quality of the micro grooves is poor. Figure 4 In (c), the scanning spacing of sample No. 11 is too small, causing the liquid metal in the middle remelting expansion zone to overflow to both sides, resulting in poor micro-groove quality.

[0080] In summary, in this embodiment, by designing an orthogonal experiment of the micro-groove SLM preparation process parameters, the effects of SLM core parameters: laser power, scanning speed and scanning spacing on the preparation of high-quality micro-groove structure were explored respectively. Finally, the optimal process parameters for SLM preparation of a minimum 200μm micro-groove structure were obtained: laser power of 275W, scanning speed of 1250mm / s, scanning spacing of 100μm, powder thickness of 30μm, and the printing direction is 90° to the horizontal direction.

[0081] In this embodiment, high-pressure gas is used to perform preliminary flushing on the SLM-molded metal part to remove metal powder and dust on the surface of the SLM-molded metal part;

[0082] Use a steel brush to preliminarily clean the loose powder and dust on the surface of the workpiece after etching;

[0083] The purpose of pickling in this embodiment is to remove powder sticking on the sample surface and prevent excessive corrosion of micro texture. In this embodiment, after optimizing the SLM process parameters, although a micro groove structure with good continuity and relatively complete structure can be obtained, the problem of powder sticking and spheroidization on the surface cannot be solved by optimizing the SLM process parameters alone. In actual production, SLM formed workpieces often need to be post-processed on their surfaces to improve their surface quality.

[0084] The method used in this embodiment is to perform the double acid etching (DAE) process and ultrasonic surface treatment simultaneously. The specific instruments and conditions used in the operation are as follows: Figure 5 shown.

[0085] The pickling solutions used in the pickling part of this embodiment are: hydrofluoric acid (HF) single acid pickling solution and hydrofluoric acid (HF) + nitric acid (HNO 3 ) double acid pickling solution. The types and composition ratios of different pickling solutions are shown in Table 3, wherein pickling solution 1 is used as a control group and is only cleaned with deionized water, pickling solutions 2 to 5 are single acid pickling systems, and pickling solution 6 is a double acid pickling system.

[0086] Table 3 Pickling liquid types and their composition ratios

[0087]

[0088] This example explores the effects of the core pickling parameters, such as acid concentration ratio and pickling time, on the micro-groove structure prepared by SLM. By analyzing them, the optimal pickling parameters most suitable for the micro-groove structure of this subject are obtained.

[0089] (1) Effect of pickling solution concentration ratio on microgroove structure

[0090] The common pickling solution used for solid titanium in the factory is currently divided into single acid and double acid systems, and the core components of the two are hydrofluoric acid, which is used to chemically react the titanium alloy surface to achieve the purpose of efficiently removing the unmelted or semi-melted particles of the titanium alloy surface burrs and adhesion. The difference between the two is mainly whether to add nitric acid, which can promote the hydrogen embrittlement of parts in the titanium and hydrofluoric acid reaction process, which has a huge impact on the micro-groove structure. When nitric acid reacts with titanium, a dense oxide film will be formed on the titanium surface, and the sample surface will be passivated, which will also help prevent the micro-groove structure from excessive corrosion while reducing the hydrogen embrittlement phenomenon. Therefore, the present embodiment will adopt the double acid system pickling solution to pickle the micro-groove cooling channel.

[0091] In this embodiment, 1%, 3%, 5%, and 10% hydrofluoric acid were selected for the test. Since the above reaction is an endothermic reaction, in order to increase the reaction speed and make the pickling of the micro-groove surface more uniform, firstly, the polytetrafluoroethylene beaker containing the pickling solution is placed in the ultrasonic cleaner, the ultrasonic vibration is started, and the water bath heating temperature is set to 35°C. After the temperature of the pickling solution reaches the set temperature, the samples are respectively placed in the pickling solutions 1-5 for ultrasonic cleaning for 3 minutes, and then the samples are taken out of the pickling solution and placed in deionized water for ultrasonic cleaning to remove the residual pickling solution on the surface and then observed. Fig.14 The macroscopic morphology of the 200μm micro-groove surface after pickling with different pickling solutions. Fig.14 Surface morphology of the samples after pickling with different pickling solutions: Fig.14 (a) is pickling solution 1, Fig.14 (b) is pickling solution 2, Fig.14 (c) in the above is pickling solution 3, Fig.14 (d) in the above is pickling solution 4, Fig.14 (e) in the above is pickling solution 5. Fig.14 As can be seen in (a), deionized water cannot remove the sticky powder and spheroidized particles on the surface of the sample, so the surface quality of the SLM-prepared sample is extremely poor, and only the designed micro-groove structure can be vaguely seen. Fig.14 The surface powder and spheroidized particles in (b) and (c) are greatly reduced, and the outline of the designed micro-groove structure gradually becomes clear. When the hydrofluoric acid concentration increases to 5%, Fig.14In (d), it can be clearly seen that the designed micro-groove structure begins to be damaged and the micro-groove structure is no longer continuous and complete. When the hydrofluoric acid concentration is directly increased to 10%, Fig.14 The surface color of the sample (e) changes and starts to turn yellow and white, indicating that the micro-groove structure is over-corroded and oxidized seriously. Based on the above discussion, this embodiment selects 5% hydrofluoric acid concentration as the hydrofluoric acid concentration for post-acid treatment of the micro-groove cooling channel.

[0092] Figure 6 The surface morphology of the 200μm micro-groove structure under different pickling times: Figure 6 (a) is not pickled. Figure 6 (b) is pickling for 2 minutes. Figure 6 (c) is pickling for 4 minutes. Figure 6 (d) in the figure is pickled for 6 minutes. Figure 6 As shown in (b) in the figure, a large amount of powder sticking to the sample surface was removed within 2 minutes of pickling, but a large amount of metal powder remained at the bottom of the groove. At the same time, the surface of the micro-groove structure was covered with many pits due to the shedding of metal powder, and the edges of the pits were relatively sharp, and the overall micro-groove surface roughness was relatively large. As the pickling time increased, at 4 minutes, the surface roughness of the micro-groove structure was Figure 6 In (c), the metal powder in the micro-groove structure is basically cleaned up. At the same time, due to the corrosion of the pickling solution, the sharp edges left after the metal powder falls off are also passivated. The size of the micro-groove structure is measured and it is found that the micro-groove structure is basically consistent with the design size at this time, indicating that the micro-groove structure is not corroded at this time. However, when the pickling time continues to increase to 6 minutes, Figure 6 As can be seen in (d), the groove spacing of the micro-groove structure is enlarged and the rib structure size is reduced, indicating that the micro-groove structure has been over-corroded.

[0093] In summary, after the above tests, the optimal process parameters for pickling of the closed cooling channel with a minimum micro-groove structure of 200 μm in this embodiment are determined as follows: the pickling liquid adopts a double acid system, HF-HNO 3 The concentration ratio is 5%:20%, heated in a 35°C water bath, ultrasonic assistance is added, and the pickling time is 5 minutes. Fig.15 The 200μm micro-groove structure morphology after the optimal pickling process parameters are used for the complete cooling channel structure. Fig.15 It can be seen that the pickling effect is better and can meet the use requirements.

[0094] In this embodiment, the pickling time should not be too short, otherwise the pickling will not be thorough, and powder will remain on the surface of the micro-texture, affecting the drag reduction effect; at the same time, as the pickling time is prolonged, the pickling liquid will cause serious corrosion to the micro-texture structure while removing sticky powder and surface micro-burrs. However, due to the addition of nitric acid, double-acid pickling forms an oxide film on the surface of the sample, thereby effectively protecting the main body of the texture and preventing damage to the texture while removing surface micro-burrs.

[0095] The sample was taken out with tweezers and dried to obtain a micro-textured regenerated cooling channel sample.

[0096] Energy spectrum analysis was performed on the rectangular groove structure surface of the sample prepared before pickling in Example 1, the sample prepared after double acid pickling in pickling solution 6, and the sample after single acid pickling in pickling solution 4 in Example 1. The results of the energy spectrum analysis are shown in Table 4. Figure 7 This is the EDS layered image of the sample that was not pickled in Example 1. Figure 8 This is the EDS layered image of the sample after pickling with pickling solution 6 in Example 1. From the above results, it can be seen that the common elements and contents of the unpickled and pickled samples after energy spectrum are: Ti, AI, Zr, Mo, V, and the contents of these elements are roughly consistent with the contents recommended by the technical standards, indicating that the credibility of the energy spectrum results is high. In addition, fluorine was detected on the surface of the pickled sample, which is due to the presence of hydrofluoric acid in the pickling solution used during pickling. Compared with the surface elements of the unpickled sample, the carbon and oxygen elements on the surface of the sample after pickling decreased significantly, indicating that pickling can significantly remove the surface oxides generated during the SLM process.

[0097] Table 4 Energy spectrum analysis results of samples in Example 1 and Comparative Example 1

[0098]

[0099] Example 2

[0100] This embodiment provides a method for manufacturing micro-texture of the inner wall of a cooling channel based on SLM integrated processing of micro-texture regeneration, comprising the following steps:

[0101] In this example, three samples with different micro-groove sizes were prepared.

[0102] Sample 1: microgroove dimensions: p = 400 μm, s = h = 250 μm;

[0103] Sample 2: microgroove dimensions: p = 400 μm, s = h = 350 μm;

[0104] Sample 3: microgroove dimensions: p = 400 μm, s = h = 450 μm;

[0105] Among them, blank sample: smooth wall.

[0106] The SLM process parameters are: laser power 275W, scanning speed 1250mm / s, scanning spacing 100μm, powder thickness 30μm, and the printing direction is 90° to the horizontal direction. Pickling operation: The pickling solution uses a double acid system, HF-HNO 3 The concentration ratio is 5%:20%, the mixture is heated in a water bath at 35°C, ultrasonic waves are added to assist, and the pickling time is 5 minutes. The remaining operations are the same as those in Example 1.

[0107] The samples with different groove wall surfaces prepared in Example 2 (samples 1 to 3 and blank samples) were subjected to a circulating water tunnel test. The circulating water tunnel test was conducted using a circulating water tunnel platform. The device diagram of the circulating water tunnel platform is shown in FIG. Fig. 9 In the circulating water tunnel platform of the circulating water tunnel experiment: 1 is the test section; 2 is the water tank; 3 is the insulation layer; 4 is the heating plate; 5 is the wall to be heated; 6 is the thermocouple; 7 is the temperature transmitter; 8 is the wall to be insulated; 9 is the differential pressure transmitter; 10 is the electromagnetic flowmeter; 11 is the centrifugal pump; 12 is the motor inverter; 13 is the inlet contraction section; 14 is the outlet expansion section.

[0108] Fig. 9 The schematic diagram of the multifunctional circulating water tunnel is shown in Figure 1. The circulating water tunnel consists of a test pipe section 1, a pump 11, a flow meter 10, a differential pressure transmitter 9, a temperature transmitter 7, a contraction pipe section 13, an expansion pipe section 14, and a water tank 2. The middle test section has a spacing of 500 mm, and a single cooling channel or parallel multi-cooling channel specimen can be installed according to the experimental needs, and can also be replaced with a PIV transparent test pipe section.

[0109] A heating plate was installed on the lower wall (heating wall) of the test section to simulate the single-sided heating condition of the regenerative cooling channel (heating temperature was 200°C). Five thermocouples were arranged at equal intervals along the flow direction in the center of the upper wall (insulating wall) of the cooling channel of the test section, and their average value was calculated to evaluate the thermal protection performance of the test pipe section. A layer of thermal insulation cotton was wrapped on the outermost layer of the entire test pipe section to reduce the interference of heat loss and ambient temperature on the test results. Ordinary tap water was used as the coolant, and the inlet water temperature was controlled at 24±0.5°C.

[0110] The experimental Reynolds number is D h is the characteristic length, p is the fluid density, U is the fluid flow velocity, and v is the fluid dynamic viscosity.

[0111] Where: D h is 4.

[0112] p is 1000kg / m 3 .

[0113] U is 0.38, 0.99, 1.54, 1.96, 2.42m / s.

[0114] v is 0.001Pa×s.

[0115] Through the insulation wall temperature, see Fig.10 The thermal protection capability of the regenerative cooling channel is shown in the analysis. Under the condition of 200°C heating of the outer wall, the insulation surface temperature of the micro-grooved cooling channel is always lower than that of the smooth wall cooling channel, and with the increase of the No., the difference between the two gradually increases and then tends to be flat. This shows that under the technical manufacturing of this scheme, the enhanced heat exchange effect of the regenerative cooling flow is significantly enhanced under the action of micro-texture compared with the smooth channel.

[0116] From the above embodiments, it can be seen that:

[0117] 1. From the perspective of practical needs and applications, the present invention designs a method for manufacturing micro-texture on the inner wall of a micro-textured regenerative cooling channel, which can significantly improve product quality, improve processing accuracy and reduce manufacturing costs.

[0118] 2. The microchannel microtexture processed by the present invention can increase the flow rate of the coolant, increase the heat exchange coefficient between the wall and the coolant, and effectively reduce the temperature of the inner wall, which has a better cooling effect than the existing structure.

[0119] 3. The present invention forms the micro-texture in the regenerative cooling channel through SLM integrated processing, thereby achieving precise control of the cross-sectional shape of the processed micro-grooves, including the contour, micro-texture width, and micro-texture depth; and processes the surface of the microchannel to have a surface feature with a precisely controllable cross-sectional shape and a smooth bottom morphology.

[0120] 4. Traditional microfluidic channel processing microtexture methods such as laser etching process mainly achieve the purpose of microtexture processing in the Z-axis direction, while SLM integrated processing microtexture regeneration cooling channel microtexture can achieve microtexture arrangement in the X and Y axis directions, breaking the limitations of traditional methods.

[0121] 4. The present invention can improve the coolant flow rate in the cooling channel of the regenerative cooling combustion chamber and the uniformity of the temperature of the same cross section while keeping the total coolant flow rate unchanged, thereby preventing the coolant from being overheated and vaporized at a certain place, causing local damage to the combustion chamber, and ensuring uniform and effective cooling of the regenerative cooling combustion chamber.

[0122] 5. The present invention can be quickly adapted according to the actual engine structure, and has the advantages of wide applicability, economy, convenience and significant effect, solving the problems of the existing technology with insignificant drag reduction effect and poor adaptability.

[0123] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a micro-textured regenerative cooling channel, characterized in that: The following steps are involved: A selective laser melting additive manufacturing method is used to form a downstream rectangular micro-groove on the inner wall of the regenerative cooling channel, thereby obtaining an initial micro-groove structure on the inner wall of the regenerative cooling channel; The initial micro-groove structure is pickled with a mixed acid solution under ultrasonic conditions to obtain the micro-texture regeneration cooling channel, and the mixed acid solution is a mixed acid solution of hydrofluoric acid and nitric acid.

2. The preparation method according to claim 1, characterized in that: The cross section of the downstream rectangular micro-groove is rectangular, and the groove width and groove depth of the groove are independently 200 to 500 μm; The groove spacing is 400 to 1000 μm.

3. The preparation method according to claim 1, characterized in that: The particle size of the molding powder used in the selective laser melting is 15 to 53 μm; the molding powder used in the selective laser melting is TA15 titanium alloy powder.

4. The preparation method according to claim 1 or 3, characterized in that: The selective laser melting is carried out by horizontal placement of the regenerative cooling channel and vertical processing; The conditions for the selective laser melting include: the laser type is a continuous laser, the scanning path is a zigzag path, the thickness of the powder layer is 0.02-0.08 mm, the diameter of the laser spot is 80 μm, and the processing angle is 90°.

5. The preparation method according to claim 4, characterized in that: The power of the continuous laser is 150-300W, the scanning speed is 800-1400mm / s, and the scanning interval is 0.06-0.16mm.

6. The preparation method according to claim 1, characterized in that: The mixed acid solution of hydrofluoric acid and nitric acid comprises HF, HNO3 and water; in the mixed acid solution of hydrofluoric acid and nitric acid: the mass percentage of HF is 1-10%, and the mass percentage of HNO3 is 10-20%.

7. The preparation method according to claim 1 or 6, characterized in that: The ultrasonic conditions include: the ultrasonic power is 400-500W, the frequency is 40-60kHz; the pickling temperature is 20-60°C, and the time is 3-5min.

8. The preparation method according to claim 1, characterized in that: After the initial micro-groove structure is obtained and before the pickling, the method further includes: flushing the initial micro-groove structure, wherein the flushing is performed using high-pressure gas, and the pressure of the high-pressure gas is 0.3-0.6 MPa.

9. The micro-textured regenerative cooling channel prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The inner wall surface of the micro-textured regenerative cooling channel has an integrated downstream rectangular micro-groove.

10. Use of the micro-textured regenerative cooling channel according to claim 9 in thermal protection of an engine combustion chamber.

Citation Information

Patent Citations

  • Micro reaction tube with complex internal channel structure and manufacturing method of micro reaction tube

    CN108837782A

  • Selective laser melting forming and post-treatment method for thin-wall interlayer cooling structure

    CN112496341A

  • Integrated additive manufacturing method for dissimilar metal closed runner

    CN115415543A

  • Cooling flow channel structure for directional liquid transportation

    CN214850864U

  • Cooled wall structure for the hot gas parts of a gas turbine and method for manufacturing such a structure

    EP2685170A1

Cited By

  • Method for additive manufacturing and inner surface treatment of inner runner part

    CN120861845A