Laser welding method
By using multiple welding methods of primary welding preheating and secondary welding in laser welding, preheating and high-energy density welding is performed using laser beams with positive and negative defocusing amounts, the problem of insufficient melting depth of small power lasers is solved. Welding strength improvement and cost savings are achieved.
Patent Information
- Application Number
- CN202411270363.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The welding melting depth of low-power lasers cannot meet specific requirements, and high-power equipment is costly, and existing methods require changing the size of welding parts to increase the melting depth.
The multiple welding methods of primary welding preheating and secondary welding are adopted, and the laser beams with positive defocus and negative defocus are used for preheating and high-energy density welding respectively to increase the welding melting depth and without changing the size of the welding parts. Improve welding strength under the premise of
It realizes a significant increase in welding depth and increase in welding strength without changing the size of welding parts, and reduces equipment costs without changing the size of welding parts.
Smart Images

Figure CN118926695A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of laser welding, and in particular to a laser welding method. Background Art
[0002] Laser welding is an efficient and precise welding method that uses a high energy density laser beam as a heat source.
[0003] IPG YLS-4000 is a sealed cabinet laser with a maximum welding power of 4KW. Limited by the maximum welding power, its welding penetration is generally less than 4mm. If you want to increase the welding penetration, one way is to use a higher power laser welding device, but the equipment cost is extremely high. There are also some methods that can use vacuum chamber negative pressure welding methods; or reserve weld gaps and use composite welding methods, but both require changing the size of the welded parts and cannot meet the processing requirements of some parts. Summary of the invention
[0004] The present application provides a laser welding method, which can increase the welding penetration and improve the welding strength without changing the size of the workpiece to be welded by using low-power laser welding equipment, thereby greatly saving equipment costs.
[0005] To achieve the above objectives, the present application provides a laser welding method, comprising:
[0006] Pre-treat the workpiece to be welded and join the welding edges;
[0007] A first defocusing amount is used to perform a welding preheating on the welding edge of the workpiece to be welded, and the power of the welding preheating is a first preset power;
[0008] A second defocusing amount is used to perform secondary welding on the welding edge of the workpiece to be welded, and the power of the secondary welding is a second preset power;
[0009] Among them, the first defocus amount is a positive defocus amount, the second defocus amount is a negative defocus amount, and the first preset power is less than the second preset power.
[0010] In some embodiments, the first preset power is 3.2±0.2 KW, and the second preset power is 3.8-4.0 KW.
[0011] In some embodiments, the first defocus amount is +3 mm, and the welding speed of the primary welding preheating is 18 mm±3 / s.
[0012] In some embodiments, an absolute value of the second defocus amount is greater than or equal to half of a target welding penetration.
[0013] In some embodiments, the second defocus amount is -3.5 mm, and the welding speed of the secondary welding is 12 mm±2 / s.
[0014] In some embodiments, the steps of pre-treating the workpieces to be welded and joining the weld edges include:
[0015] Grind the welding edges of the workpieces to be welded;
[0016] Ultrasonic cleaning of workpieces to be welded;
[0017] Use welding fixture to clamp and fix the workpiece to be welded.
[0018] In some embodiments, the angle between the incident laser of the primary welding preheating and the secondary welding and the welding edge of the workpiece to be welded is 5-6°.
[0019] In some embodiments, the primary welding preheating and the secondary welding are welding without shielding gas.
[0020] In some embodiments, during the primary welding preheating and the secondary welding process, the shielding gas is heated and blown onto the surface of the workpiece to be welded.
[0021] In some embodiments, after the step of performing secondary welding on the welding edge of the workpiece to be welded using the second defocus amount, the step further includes:
[0022] Inspect and treat the weld surface.
[0023] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art: after the surface of the workpiece to be welded is processed and the welding edge is spliced, the welding of the workpiece to be welded adopts a multiple welding method of primary welding preheating and secondary welding. During the welding process, the workpiece to be welded is welded once with a positive defocus amount and a smaller first preset power to achieve preheating of the welding edge, increase the temperature of the welding edge of the workpiece to be welded, thereby cooperating with the secondary welding to increase the energy density at the welding edge of the workpiece to be welded, which helps to increase the welding penetration; in addition, the secondary welding adopts a negative defocus amount and is welded with a larger second preset power, so that the focus of the laser beam falls on the first distance below the surface of the workpiece to be welded, the internal power density is higher than the surface, it is easy to form stronger melting and vaporization, so that the light energy is transmitted deeper into the material, thereby obtaining greater penetration; the preheating of the primary welding makes the energy density distribution of the workpiece to be welded located above and below the focus of the laser beam of the secondary welding similar, that is, a welding penetration close to or even greater than twice that of the conventional welding method is generated. There is no need to update the high-power laser welder, which reduces the equipment cost, and there is no need to change the size of the workpiece to be welded, which meets the processing requirements of customers. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplified descriptions do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and unless otherwise stated, the figures in the drawings do not constitute proportional limitations.
[0027] Figure 1 A flow chart of a laser welding method provided in an embodiment of the present application;
[0028] Figure 2 A welding schematic diagram of a welding method for the workpiece to be welded;
[0029] Figure 3 A welding schematic diagram of another welding method for the workpiece to be welded.
[0030] Description of reference numerals:
[0031] 10- workpiece to be welded; 20- laser beam. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0033] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplification and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed.
[0034] For ease of description, spatial relative terms may be used herein to describe the relative positional relationship or movement of one element or feature relative to another element or feature as shown in the figure, such as "inside", "outside", "inner side", "outer side", "below", "below", "above", "above", "front", "back", etc. Such spatial relative terms are intended to include different orientations of the device in use or operation in addition to the orientation depicted in the figure. For example, if the device in the figure undergoes a position flip or a posture change or a motion state change, then these directional indications also change accordingly, for example: an element described as "below other elements or features" or "below other elements or features" will subsequently be oriented as "above other elements or features" or "above other elements or features". Therefore, the example term "below..." may include both upper and lower orientations. The device may be otherwise oriented (rotated 90 degrees or in other directions) and the spatial relative descriptors used herein are interpreted accordingly.
[0035] In order to solve the technical problems in the prior art that the welding penetration of small-power lasers cannot reach a specific penetration depth and the cost of high-power equipment is relatively high; the present application provides a laser welding method, which can increase the welding penetration depth and improve the welding strength without changing the size of the workpiece 10 to be welded by using small-power laser welding equipment, thereby greatly saving equipment costs.
[0036] The laser welding method provided in the embodiment of the present application is as follows Figure 1 As shown, including:
[0037] Step S10: pre-treating the workpiece 10 to be welded and splicing the welding edges;
[0038] Step S20: preheating the welding edge of the workpiece 10 to be welded by using a first defocusing amount, and the power of the first welding is a first preset power;
[0039] Step S30: performing secondary welding on the welding edge of the workpiece 10 to be welded by using a second defocusing amount, and the power of the secondary welding is a second preset power;
[0040] Among them, the first defocus amount is a positive defocus amount, the second defocus amount is a negative defocus amount, and the first preset power is less than the second preset power.
[0041] The defocus refers to the distance between the focus of the laser beam 20 and the surface of the workpiece 10 to be welded. The power density at the center of the spot at the laser focus is the highest, and it is easy to evaporate and form a hole. On each plane away from the laser focus, the power density distribution is relatively uniform.
[0042] Positive defocus refers to the distance at which the focus of the laser beam 20 is located above the surface of the workpiece 10 to be welded; negative defocus refers to the distance at which the focus of the laser beam 20 is located below the surface of the workpiece 10 to be welded. When the distances between the positive and negative defocus planes and the welding plane are equal, the power density on the corresponding planes is roughly the same in theory, but the actual weld penetration and shape are different. When the defocus is negative, the internal power density of the material is higher than the surface, which easily forms stronger melting and vaporization, allowing the light energy to be transmitted deeper into the material, thereby obtaining greater penetration.
[0043] In step S10, the method of pre-treating the workpiece 10 to be welded includes grinding the side surfaces of the welding edges of the workpiece 10 to be welded to ensure the flatness of the joints of different welded workpieces and avoid irregular gaps after the welding edges are spliced, thereby ensuring the uniformity of the energy transfer of the laser beam 20 so as to control the shape and depth of the molten pool.
[0044] The pretreatment method also includes ultrasonic cleaning of the polished workpiece 10 to be welded to remove the grinding debris and impurities on the surface of the workpiece 10 to be welded, and improve the energy transmission of the laser beam 20. Then, the welding edges of different workpieces 10 to be welded are spliced according to the welding requirements, and the workpieces 10 to be welded are clamped and fixed with a welding fixture so that the welding edges of the workpieces 10 to be welded can be welded later.
[0045] In step S20, a laser beam 20 with a first defocus amount is used to perform a welding preheating on the spliced welding edge. The first defocus amount is a positive defocus amount, that is, the focus of the laser beam 20 is located above the surface of the workpiece 10 to be welded. The primary welding preheating is performed at a first preset power, which is less than the second preset power and less than the maximum power of the laser. The main purpose of the primary welding preheating is to preheat and raise the temperature of the welding edge to facilitate the secondary welding to increase the energy density at the welding edge and form a greater welding penetration.
[0046] In step S30, a laser beam 20 with a second defocus amount is used to repeatedly weld the welding edge that has been preheated for the first welding. Since the welding edge has a certain temperature after the first welding preheating, the secondary welding laser beam 20 can raise the welding edge to a higher temperature and transfer it to a deeper depth from the surface. The second defocus amount of the secondary welding adopts a negative defocus amount. The focus of the laser beam 20, that is, the part with the highest energy density, is below the surface of the workpiece 10 to be welded. The laser beam 20 can be transferred to a position deeper than the surface of the workpiece 10 to be welded, and cooperate with the first welding preheating to achieve a significant increase in the welding penetration.
[0047] In this application, a YLS-4000 laser is used to weld three workpieces 10 (plates) according to Figure 2 Corner joint as shown or as per Figure 3The T-joint welding method shown is used to illustrate that the maximum welding power of the YLS-4000 laser is 4.0KW, and the welding penetration depth that can be achieved is generally around 4mm. By using the laser welding method provided in this application, the welding penetration depth can be increased to greater than or equal to 7mm without changing the size of the workpiece 10 to be welded and the welding edge gap, thereby improving the welding strength.
[0048] In some embodiments, the welded parts are made of 4-6 mm metal sheets, such as 5 mm thick metal sheets. The first preset power of the primary welding preheating is 3.2±0.2KW, the first defocusing amount is +3mm, and the welding speed of the primary welding preheating is 18±3mm / s.
[0049] In some embodiments, the second preset power of the secondary welding is 3.8-4.0KW, the absolute value of the second defocus is greater than or equal to half of the target welding penetration, if the target welding penetration is h (h>0), then the absolute value of the second defocus is greater than or equal to h / 2, that is, the second defocus is less than -h / 2, and the welding speed of the secondary welding is 12±2mm / s. The second defocus is -3.5mm, and the welding speed of the secondary welding machine is 12±2mm / s.
[0050] Since part of the heat energy is lost after the laser beam 20 is irradiated onto the surface of the workpiece 10 to be welded, in order to reduce the energy loss of the laser beam 20, the present application adopts multi-level welding, that is, firstly, a laser beam 20 with a first preset power is used to preheat the welding edge of the workpiece 10 to be welded with a first defocus amount and a first welding speed, and then a laser beam 20 with a second preset power is used to perform final welding with a second defocus amount and a second welding speed, and the second welding speed is less than the first welding speed.
[0051] Corresponding to the welding of three metal sheets with a thickness of 5mm in the form of corner joints or T-joints, the parameters of YLS-4000 laser welding used in this application are preferably set as follows: the power of the first welding is 3.2KW, the defocus is +3mm, and the welding speed v=18mm / s; the power of the second welding is 4.0KW, the defocus is -3.5mm, and the welding speed vv=12mm / s. After the welding parameters and welding trajectory are adjusted, the three metal sheets are cleaned with an ultrasonic cleaner, and then the three metal sheets are spliced according to the welding requirements and positioned and clamped with a fixture, and finally automatically welded into shape. From the appearance of the welding surface, the welding quality meets the ISO13919 welding standard. From the results of multiple sectioning, the welding penetration has reached 7.29mm, 7.84mm, and 7.54mm, respectively, that is, the IPG YLS-4000 laser can meet a penetration of more than 7mm.
[0052] When the laser beam 20 is used to weld the welding edge of the workpiece 10 to be welded, the incident laser and the welding edge of the workpiece 10 to be welded are as follows: Figure 2 or Figure 3 There is an angle between the incident laser and the vertical surface of the plate. The smaller the angle, the deeper the welding penetration. Through theoretical calculation and practical verification, when the laser beam 20 does not burn the surface of the workpiece 10 in the vertical direction, the angle between the incident laser and the vertical surface of the workpiece 10 to be welded is set to 5-6°. For example, the angle between the incident laser and the vertical surface of the workpiece 10 to be welded can be 5°, 5.2°, 5.4°, 5.6°, 5.8° and 6°.
[0053] The shielding gas is mainly used to protect the focusing lens from the sputtering of metal vapor and liquid droplets, and to blow away the barrier effect of the plasma cloud on the laser beam 20. However, the shielding gas will take away some heat during laser welding, reducing the welding penetration. At the same time, for workpieces with poor welding performance, adding shielding gas will accelerate the cooling rate of the weld surface, increase the hardening tendency of the material, and make cracks more likely to occur. In order to reduce heat loss and increase welding penetration, it is necessary to reduce the heat loss caused by the shielding gas.
[0054] The welding method adopted in one embodiment of the present application is non-shielded gas welding, that is, during the primary welding preheating and secondary welding process, no shielding gas is blown onto the surface of the workpiece 10 to be welded, thereby reducing the heat loss caused by the cooling of the shielding gas and achieving the purpose of increasing the welding penetration.
[0055] Another embodiment of the present application adopts a welding method as follows: during the primary welding preheating and secondary welding processes, the shielding gas is heated and then blown onto the surface of the workpiece 10 to be welded; by heating the shielding gas, the temperature of the shielding gas is increased, and the temperature difference between the shielding gas and the surface of the workpiece 10 to be welded is reduced, thereby reducing the heat loss at the welding edge of the workpiece 10 to be welded caused by the shielding gas, which can increase the welding penetration to a certain extent.
[0056] In order to ensure the welding qualification rate, the laser welding method provided in the present application also includes inspecting and processing the weld surface formed after the secondary welding to ensure that the weld meets the welding standards. The processing of the weld includes grinding the weld surface or performing filler welding on the weld.
[0057] It should be understood that the terms used herein are only for the purpose of describing specific example embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "an" and "said" as used herein may also be meant to include plural forms. The terms "include", "comprise", "contain", and "have" are inclusive, and therefore specify the existence of stated features, steps, operations, elements and / or parts, but do not exclude the existence or addition of one or more other features, steps, operations, elements, parts, and / or combinations thereof. The method steps, processes, and operations described herein are not interpreted as necessarily requiring them to be performed in the specific order described or illustrated, unless the execution order is clearly indicated. It should also be understood that additional or alternative steps may be used.
[0058] Although the terms first, second, third, etc. can be used in the text to describe multiple elements, components, regions, layers and / or sections, these elements, components, regions, layers and / or sections should not be limited by these terms. These terms can only be used to distinguish an element, component, region, layer or section from another region, layer or section. Unless the context clearly indicates, terms such as "first", "second" and other numerical terms do not imply order or sequence when used in the text. Therefore, the first element, component, region, layer or section discussed below can be referred to as the second element, component, region, layer or section without departing from the teaching of the example embodiments.
[0059] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A laser welding method, It is characterized in that include: Pre-treat the workpiece to be welded and join the welding edges; A first defocusing amount is used to perform a welding preheating on the welding edge of the workpiece to be welded, and the power of the welding preheating is a first preset power; A second defocusing amount is used to perform secondary welding on the welding edge of the workpiece to be welded, and the power of the secondary welding is a second preset power; Wherein, the first defocus amount is a positive defocus amount, the second defocus amount is a negative defocus amount, and the first preset power is less than the second preset power; The angle between the incident laser of the primary welding preheating and the secondary welding and the welding edge of the workpiece to be welded is 5-6°; During the primary welding preheating and the secondary welding process, the shielding gas is heated and blown onto the surface of the workpiece to be welded.
2. The laser welding method according to claim 1, It is characterized in that The first preset power is 3.2±0.2KW, and the second preset power is 3.8-4.0KW.
3. The laser welding method according to claim 1, It is characterized in that The first defocus amount is +3 mm, and the welding speed of the primary welding preheating is 18±3 mm / s.
4. The laser welding method according to claim 1, It is characterized in that An absolute value of the second defocus amount is greater than or equal to half of a target welding penetration.
5. The laser welding method according to claim 4, It is characterized in that The second defocus amount is -3.5 mm, and the welding speed of the secondary welding is 12±2 mm / s.
6. The laser welding method according to claim 1, It is characterized in that The steps of pre-treating the workpiece to be welded and joining the welding edges include: Grind the welding edges of the workpieces to be welded; Ultrasonic cleaning of workpieces to be welded; Use welding fixture to clamp and fix the workpiece to be welded.
7. The laser welding method according to claim 1, It is characterized in that After the step of performing secondary welding on the welding edge of the workpiece to be welded using the second defocus amount, the following step is further included: Inspect and treat the weld surface.
Citation Information
Patent Citations
Low-alloy high-strength steel laser composite weld hardness control method
CN101362255A
Method for removing aluminum alloy laser welding air holes
CN103862178A
Method for laser beam welding for TiAl alloy
CN107552961A
Laser welding method and system
CN109967877A
Laser penetration welding technology for aluminum alloy medium-thick panel
CN110216375A