Ultraviolet-resistant spraying-free composite material photovoltaic frame profile and one-time pultrusion method thereof

Through the one-time pultrusion method of composite photovoltaic frame profiles with inner yarn and aromatic polyurethane resin and outer matt cloth and aliphatic resin, the problem of subsequent processing and spraying in the prior art is solved, and high efficiency and low The cost of UV resistance and mechanical properties reduces production costs and time costs.

CN118927729APending Publication Date: 2024-11-12TAISHAN FIBERGLASS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410992443.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the production process of existing composite photovoltaic frame profiles, subsequent treatment and spray coating are required to achieve ultraviolet resistance, resulting in low yield and high production costs, and the wastewater and waste gas generated during the spraying process increases the difficulty of treatment.

Method used

UV-resistant spray-free composite photovoltaic frame profile with yarn and aromatic polyurethane resin composite and its primary pultrusion molding method is adopted, through pre-drying, plasma treatment and secondary The curing zone immerse the glue to form the profile to avoid subsequent treatment and spraying.

Benefits of technology

It achieves UV resistance without subsequent processing and spraying, improves yield and reduces production costs, saves time and production costs, and ensures the mechanical properties and UV aging resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927729A_ABST
    Figure CN118927729A_ABST
Patent Text Reader

Abstract

The invention discloses an ultraviolet-resistant spraying-free composite material photovoltaic frame profile and a one-time pultrusion method thereof, and the one-time pultrusion method comprises the following steps: step 1, pre-drying pure yarns by a drying device under the traction of a traction device, then carrying out primary impregnation, and carrying out curing molding by a No.1 mold to form a profile blank; (2) the profile blank is treated through plasma equipment, surface demolding components and other grease substances are removed, and the profile blank enters a coating area; (3) the felt cloth wraps the surface of the profile blank at the pre-forming position, then is infiltrated by aliphatic resin, and enters a secondary curing area together with the profile blank to be cured into a final profile through a second mold; and the final product is chopped into a proper size according to requirements. The profile produced through the method does not need to be subjected to subsequent treatment and spraying, the requirement for the ultraviolet aging resistance of the product can be met, the yield is increased, and the production and time cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of pultrusion technology, specifically to a UV-resistant spray-free composite photovoltaic frame profile and a one-step pultrusion molding method thereof. Background Art

[0002] Composite photovoltaic frame profiles, the main production method in the industry at present is to use glass fiber or glass fiber felt cloth and epoxy, polyurethane or unsaturated resin to fully impregnate, and then pultrusion solidification molding. After molding, in order to meet the UV resistance requirements during use, the profiles need to be further post-processed, such as grinding, polishing, dust removal, flame burning, etc., and finally spray coating on the surface of the profile to achieve the purpose of UV resistance. Such operation greatly reduces the yield rate, increases time and production costs, and the large amount of wastewater and waste gas generated during the spraying process also increases the difficulty of subsequent treatment of enterprises; another way is that the frame profile products are completely pultruded using aliphatic resins, but aliphatic resins are more expensive than aromatic resins. Although this production method does not require subsequent spraying treatment, the production cost is very high, which greatly increases the pressure on production and sales. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a UV-resistant, spray-free composite photovoltaic frame profile and a one-time pultrusion molding method thereof. The profile produced by this method does not require subsequent treatment and spraying, which can not only meet the product's UV aging resistance and improve the yield, but also reduce production costs. In addition, the production method provided by the present invention does not require post-processing and spraying, thereby saving time costs compared with traditional manufacturing methods.

[0004] As the first aspect of the present invention, there is provided a UV-resistant spray-free composite material photovoltaic frame profile, comprising an inner layer and an outer layer coated on the outside of the inner layer, wherein the inner layer is a composite of yarn and aromatic polyurethane resin, and the outer layer is a composite of felt cloth and aliphatic resin.

[0005] As a second aspect of the present invention, a one-time pultrusion molding method of the UV-resistant spray-free composite photovoltaic frame profile is also provided, comprising the following steps:

[0006] Step ①, the yarn is pre-dried by a drying device under the traction of a traction device, and then initially dipped in glue and cured in a primary curing zone to form a profile blank;

[0007] Step ②, the profile blank is treated by plasma equipment to remove surface demoulding components and other grease substances, and enters the coating area;

[0008] Step ③, the felt cloth is coated on the surface of the profile blank and then impregnated with aliphatic resin, and then enters the secondary curing zone together with the profile blank to be cured into the final profile.

[0009] Among them, in step ①, the yarn must be passed through an oven before being dipped in glue, with a pre-drying temperature of 95-135°C to remove excess surface moisture from the fiber. Reducing the moisture content of the yarn can greatly improve the appearance of the product, reduce defects, and provide protection for subsequent production.

[0010] Wherein, in step ①, the resin for dipping is an aromatic epoxy resin or an aromatic polyurethane resin or an unsaturated resin. The beneficial effect of using such resin is that the production cost can be reduced while ensuring the mechanical properties of the product.

[0011] Among them, in step ①, the wall thickness of the mold in the primary curing zone is 0.1-1.0 mm smaller than the wall thickness of the mold in the secondary curing zone. The effect of such a design is that the profile blank needs to be coated later, and after the coating is completed, its overall size meets the use requirements. In the embodiment of the present invention, the mold in the primary curing zone is mold No. 1, and the mold in the secondary curing zone is mold No. 2.

[0012] Among them, in step ②, the profile blank is subjected to plasma surface treatment by plasma equipment to remove surface release agents and other grease substances, which has the beneficial effect of increasing the surface energy of the profile blank, which is conducive to better bonding of the profile blank with the subsequent covering fabric.

[0013] Wherein, in step ③, the felt cloth covering the outer surface of the profile blank can be glass fiber chopped strand mat or surface mat or glass fiber axial fabric.

[0014] Among them, in step ③, the resin used for impregnating the felt cloth covering the outer surface of the profile blank must be aliphatic epoxy resin or aliphatic polyurethane resin. Its beneficial effect is that such resin has strong UV resistance.

[0015] Among them, in step ③, the felt cloth used needs to be baked with a baking lamp before dipping, and the temperature of the irradiation area of ​​the baking lamp is 80-140° C. The beneficial effect is that after baking with the baking lamp, the moisture contained in the felt cloth can be effectively removed, and the surface defects of the profile product can be reduced.

[0016] Among them, in step ③, the felt cloth is positioned and wrapped on the surface of the profile blank in the preforming area, and is cured and formed in mold No. 2 after being dipped in glue. The preforming needs to be designed for the profile blank and the felt cloth to achieve the effect of perfect coating of the profile blank surface by the felt cloth, and avoid the problem of overlapping or loose docking of the felt cloth.

[0017] Among them, in step ③, the felt cloth covering the outer surface should be connected at the profile groove position. The beneficial effect is that there will be structural adhesive and glass filling here during the subsequent use of the components, and it will not be directly exposed to the external environment. Even if there is a problem of loose connection, it will not affect the use.

[0018] Preferably, the one-time pultrusion method has a production line structure that, along the pultrusion direction, comprises, in sequence, a yarn supply area, a yarn drying area, a first glue injection area, a first molding and curing area, a profile blank plasma treatment area, a felt cloth and profile blank preforming area, a secondary glue injection area, a secondary curing area, a support and traction area, and also includes a felt cloth rack and a baking lamp area. The felt cloth is led down through the felt cloth rack, passes through the baking lamp area during its travel, and then is completely covered with the profile blank in the felt cloth and profile blank preforming area, and the two enter the secondary glue injection area together.

[0019] Compared with the prior art, the beneficial effects of the present invention include:

[0020] 1. The present invention provides a novel profile structure and a preparation method of different resin composites. The inner layer of the product is a structure in which yarn is impregnated with aromatic epoxy resin, aromatic polyurethane resin or unsaturated resin, and then covered with felt cloth, and then the surface is impregnated with aliphatic resin. The inner layer structure ensures mechanical properties, and the outer layer structure ensures UV resistance. Compared with a single resin profile of the same strength, the obtained product has a lower production cost and a shorter production cycle.

[0021] 2. The present invention uses plasma pretreatment to overcome the problem of easy stratification when different resins are compounded, and the interlayer shear strength of the obtained product is the same as that of conventional products currently on the market.

[0022] 3. In summary, the product structure and preparation method provided by the present invention have the advantages of low production cost, reliable product mechanical properties and short production cycle, and have good market prospects compared to existing products. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0024] Figure 1 It is a front view of a one-time pultrusion molding method of a UV-resistant spray-free composite material photovoltaic frame profile of the present invention; wherein 100 is a yarn supply area, 110 is a yarn drying area, 120 is a first glue injection area, 130 is a first molding and curing area, 140 is a profile blank plasma treatment area, 150 is a felt cloth and profile blank preforming area, 160 is a secondary glue injection area, 170 is a secondary curing area, 180 is a supporting traction area, 190 is a short cutting area, 200 is a felt cloth rack, and 210 is a baking lamp area;

[0025] Figure 2 is a cross-sectional view of mold No. 1 of the present invention;

[0026] Figure 3 is a cross-sectional view of mold No. 2 of the present invention;

[0027] Figure 4 is a cross-sectional view of a preformed product covered with a felt cloth and a profile blank; wherein 401 is the profile blank, and 402 is the felt cloth;

[0028] Figure 5 is a schematic diagram of plasma surface treatment;

[0029] Figure 6 601 is a schematic diagram of a cross section of a profile produced by the present invention; wherein 601 is an inner layer, and 602 is an outer layer;

[0030] Figure 7 The contact angle detection diagram of the profile blank surface before and after plasma treatment, wherein Figure a is the profile blank surface before treatment, and Figure b is the profile blank surface after treatment. DETAILED DESCRIPTION

[0031] Upon request, specific embodiments of the present invention will be disclosed herein. However, it should be understood that the embodiments disclosed herein are merely typical examples of the present invention, which may be embodied in various forms. Therefore, the specific details disclosed herein are not to be considered restrictive, but merely as a basis for the claims and as a representative basis for teaching those skilled in the art to apply the present invention in various ways in any appropriate manner in practice, including using the various features disclosed herein and in combination with features that may not be explicitly disclosed herein.

[0032] In the embodiment of the present invention, the yarn used is TCR yarn, which is produced by Taishan Fiberglass and is currently a conventional yarn type in the profile production process. Because TCR yarn can meet the mechanical performance requirements of composite products, especially the longitudinal performance requirements, and TCR yarn has a high cost performance, this method embodiment uses TCR yarn. High modulus yarn can also be used for profile production, such as HMG / S-1HM and THM-1 yarn, but such high modulus and ultra-high modulus yarns are relatively expensive. From a process perspective, high modulus and ultra-high modulus yarns can fully meet production requirements, but from a cost perspective, such yarns will increase production costs, so this patent does not recommend the use of high modulus or ultra-high modulus yarns for production.

[0033] The aromatic polyurethane resin used in the embodiment of the present invention has a model number of 1511L; 18BD298 may also be used.

[0034] The composite felt used in the embodiment of the present invention has a specification of 240g, and composite felts of specifications of 240g, 300g or 350g may also be used.

[0035] The aliphatic polyurethane resin used in the embodiments of the present invention has a model number of RP-1018A.

[0036] In one embodiment, reference Figure 1, front view of the pultrusion method. Along the pultrusion direction, there are yarn supply area 100, yarn drying area 110, first glue injection area 120, first molding and curing area 130, profile blank plasma treatment area 140, felt cloth and profile blank preforming area 150, secondary glue injection area 160, secondary curing area 170, support and traction area 180, short cutting area 190, felt cloth rack 200 and baking lamp area 210.

[0037] Furthermore, 100 TCR glass yarns are passed from the creel area 100 through the yarn guide device into the oven 110, and the temperature in the oven is set at 115°C.

[0038] The yarn then enters the first glue injection area 120 and the first curing area 130, i.e., mold No. 1. In this embodiment, the resin is an aromatic polyurethane resin, which can be selected from aromatic epoxy resin, aromatic polyurethane resin, or unsaturated resin; the curing temperature in the first curing area is zoned curing, and the temperatures are 80°C / 160°C / 190°C respectively.

[0039] After being solidified and formed in the primary solidification zone 130 , a profile blank is generated.

[0040] The profile blank continues to move along the pultrusion direction and enters the plasma treatment zone 140. Figure 5 As shown, the plasma emission device performs plasma treatment on four directions of the profile blank respectively to remove demoulding components and other grease substances on the surface of the profile blank, which will reduce the surface energy of the product and affect the subsequent coating effect.

[0041] The contact angles of the profile surface before and after plasma treatment were tested respectively. The testing equipment was a DSA25S optical contact angle measuring instrument. The specific steps were as follows:

[0042] 1. Open ADVANCE software and create a new measurement using Sessile Drop in Drop Shape;

[0043] 2. Enter the experiment name and the dripping phase (water) and surrounding phase (air) information in the test information. At the same time, fill the syringe on the instrument side with the test liquid. Repeat the contact angle experiment of pure water on the solid sample surface.

[0044] 3. Filter valid data from the experimental results.

[0045] like Figure 7 The results show that the contact angle of the profile blank surface is significantly reduced after plasma treatment. The contact angle of the profile blank surface before treatment is 108.5°, and the contact angle of the profile blank surface after treatment is 47.5°, indicating that plasma treatment increases the surface energy of the profile, which is more conducive to the subsequent coating and wetting of the profile blank surface.

[0046] Furthermore, the profile blank after plasma treatment enters the preforming area 150, or the coating area, where the profile blank 401 is coated with a felt cloth 402, such as Figure 4 As shown, the width of the felt cloth is equal to the circumference of the profile section, and the felt cloth joint is located at the profile notch. The joint is chosen here because in the actual use of the profile, the notch will be filled with glass and structural adhesive, and the uneven connection of the felt cloth here will not affect the subsequent use. The felt cloth covering the profile blank can be glass fiber chopped strand mat, surface mat or glass fiber axial fabric. Different types can be selected according to different product performance requirements.

[0047] In this embodiment, the felt cloth is selected to be a layer of composite felt weighing 240g per unit area.

[0048] The felt cloth is led down through the felt cloth rack 200 and passes through the baking lamp area during its journey. The baking temperature of the baking lamp is 110°C.

[0049] The moisture content results before and after baking with a baking lamp are shown in Table 1. Baking with a baking lamp can effectively reduce the moisture content of the felt cloth, especially for polyurethane resin. The reduction in moisture content is beneficial to reducing surface defects of the product.

[0050] Table 1 Moisture content results before and after baking with baking lamp

[0051] Serial number Moisture content of felt cloth before baking by baking lamp % Moisture content of felt cloth after baking by baking lamp % 1 0.35 0.07

[0052] After preforming, the felt cloth can be completely wrapped with the profile blank, and the two enter the secondary injection area together. The injection area uses aliphatic polyurethane resin, which is selected from aliphatic epoxy resin or aliphatic polyurethane resin; the secondary curing area, that is, mold No. 2, still uses the partitioned curing method, and the curing temperature is 100℃ / 160℃ / 190℃.

[0053] In this embodiment, if Figure 2 , Figure 3 As shown, the wall thickness of the profile used in mold No. 2 is 0.5 mm thicker than that of mold No. 1.

[0054] Product cross section Figure 6 As shown, the felt cloth is evenly coated on the surface of the profile blank. The profile wall thickness of this embodiment is 2 mm, of which the inner layer 601 is 1.5 mm thick and is a composite of yarn and aromatic polyurethane resin, and the outer layer 602 is 0.5 mm thick and is a composite of 240g felt cloth and aliphatic polyurethane resin.

[0055] In this embodiment, the bonding effect between the inner and outer layers of the profile is good, and the mechanical properties test results are shown in Table 2. The interlayer shear performance of the product is normal, and there is no delamination or bubble problem.

[0056] Table 2 Mechanical properties test results of profiles under different resin types

[0057]

[0058] In Table 2, serial numbers 1 and 2 are the main molding methods in the current composite frame industry. 1 mainly uses aromatic polyurethane and then sprays the surface with an aging-resistant coating, and 2 uses aliphatic polyurethane, which is more expensive. 3, 4, and 5 are the resin types used in the present invention. Since the resin types used for the inner layer and the outer layer are different, stratification problems are very likely to occur. The present invention uses plasma pretreatment, and the interlayer shear strength of the product is the same as that of conventional products on the market, indicating that the products produced by the present invention do not have the problem of loose interlayer bonding.

[0059] In this embodiment, the UV aging resistance of the product at 0 degree tensile performance was verified, and the results are shown in Table 3. The results show that the profile produced by the present invention has good UV resistance and can meet the actual application of the product.

[0060] Table 3 UV aging resistance verification test results

[0061]

[0062]

[0063] In the results of Table 3, the ultraviolet aging strength retention rates of Comparative Examples 1 and 3 are similar to those of the embodiment of the present invention, indicating that the present embodiment has achieved a good ultraviolet aging resistance purpose. Compared with the present invention, Comparative Example 1 has a higher cost due to the complete use of aliphatic polyurethane. The specific cost situation is shown in Table 4. The resin of the present invention can save up to 55% of the production cost. Compared with the embodiment of the present invention, in order to achieve the same ultraviolet aging resistance effect, after the pultrusion production of Comparative Example 3 is completed, the product needs to be surface polished and sprayed with an ultraviolet aging resistance coating, which increases the production process and thus increases the time cost and production cost.

[0064] Table 4 Comparison of costs of different resins

[0065] Serial number Resin Type Purchase price Yuan / kg 1 Unsaturated resin 17 2 Aliphatic polyurethane resin 50 3 Aromatic polyurethane resin 25 4 Epoxy resin 19

[0066] The cost comparison of products made of different raw materials is shown in Table 5:

[0067] Table 5 Price comparison of different resin molding products

[0068]

[0069] As can be seen from Table 5, the cost of the photovoltaic frame profile with an inner layer of aromatic polyurethane resin and an outer layer of aliphatic polyurethane resin provided by the present application is reduced by 28.4% compared with the cost of using only aliphatic polyurethane resin, and is reduced by 15.6% compared with the cost of aromatic polyurethane resin coated with an aging-resistant layer.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A UV-resistant, spray-free composite photovoltaic frame profile, It is characterized in that It comprises an inner layer and an outer layer covering the inner layer. The inner layer is compounded of yarn and aromatic polyurethane resin, and the outer layer is compounded of felt cloth and aliphatic resin.

2. A one-step pultrusion method for a UV-resistant spray-free composite photovoltaic frame profile. It is characterized in that The following steps are involved: Step ①, the yarn is pre-dried by a drying device under the traction of a traction device, and then initially dipped in glue and cured in a primary curing zone to form a profile blank; Step ②, the profile blank is treated by plasma equipment to remove surface demoulding components and other grease substances, and enters the coating area; Step ③, the felt cloth is coated on the surface of the profile blank and then impregnated with aliphatic resin, and then enters the secondary curing zone together with the profile blank to be cured into the final profile.

3. The one-step pultrusion method according to claim 2, It is characterized in that In step ①, the yarn must be baked in an oven before being dipped in glue, and the pre-baking temperature is 95-135°C.

4. The one-step pultrusion method according to claim 2, It is characterized in that In step ①, the resin used for dipping is aromatic epoxy resin, aromatic polyurethane resin or unsaturated resin.

5. The pultrusion method according to claim 2, It is characterized in that The mold wall thickness of the primary curing zone is 0.1-1.0 mm smaller than the mold wall thickness of the secondary curing zone.

6. The one-step pultrusion method according to claim 2, It is characterized in that In step ③, the felt cloth covering the outer surface of the profile blank is glass fiber chopped strand mat or surface mat or glass fiber axial fabric.

7. The one-step pultrusion method according to claim 2, It is characterized in that In step ③, the resin used to impregnate the felt cloth covering the surface of the profile blank is aliphatic epoxy resin or aliphatic polyurethane resin.

8. The one-step pultrusion method according to claim 2, It is characterized in that In step ③, the felt cloth is baked with a baking lamp before being dipped in glue, and the temperature of the irradiation area of ​​the baking lamp is 80-140°C.

9. The one-step pultrusion method according to claim 2, It is characterized in that In step ③, the felt cloth covering the outer surface is butt-jointed at the profile groove position.

10. The one-step pultrusion method according to claim 2, It is characterized in that The production line structure, along the pultrusion direction, is composed of yarn supply area, yarn drying area, first glue injection area, first molding and curing area, profile blank plasma treatment area, felt cloth and profile blank preforming area, secondary glue injection area, secondary curing area, support and traction area, and also includes a felt cloth rack and a baking lamp area. The felt cloth is led down from the felt cloth rack, passes through the baking lamp area during its travel, and then is completely covered with the profile blank in the felt cloth and profile blank preforming area, and the two enter the secondary glue injection area together.

Citation Information

Patent Citations

  • Composite plate and box body

    CN107696645A

  • Method for preforming resin injection pultrusion employing multiple resins

    CN1187157A

  • Method for adhesion of thermosetting resin-molded products

    JP2003221458A

  • Pre-impregnated composite materials with improved performance

    WO2008127556A1