Comprehensive recycling method of polarizer waste liquid
Through the concentration, acidification and heating reaction of polarizing plate waste liquid, combined with the stirring reaction of zinc-containing compounds and seed crystals, the purity and recovery of iodine element and boric acid were successfully improved, and the waste of resources and environmental pollution in the prior art was solved The problem has achieved the maximum utilization of resources.
Patent Information
- Application Number
- CN202410999081.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art cannot effectively take into account the purity and recovery rate of iodine element, resulting in waste of resources and environmental pollution.
By concentrating, acidizing and heating the polarizer waste liquid, it generates iodine vapor and condenses, combines zinc-containing compounds and seed crystals for stirring reactions, and separates iodine element, zinc borate and potassium salt and other products to achieve maximum resource utilization .
The purity and recovery rate of iodine element, boric acid and potassium salts are improved, and the utilization of resources is maximized, which has economic and environmental benefits.
Smart Images

Figure CN118929578A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste liquid recovery and treatment, and in particular to a comprehensive recovery and utilization method of polarizing plate waste liquid. Background Art
[0002] Polarizing plates are the core components of liquid crystal panels, and are mainly used to transmit and block light emitted from the backlight module. Polarizing plates are divided into three categories according to different materials: metal, iodine, and dye. Among them, due to their lower cost, iodine-based polarizing plates, which are a combination of iodine molecules and polyvinyl alcohol, have the highest market share. In the preparation process of iodine-based polarizing plates, the polyvinyl alcohol film needs to be dyed in an iodine-containing solution. The main components of this iodine-containing solution are iodine and potassium iodide. Boric acid is usually added to increase the hardness of the polyvinyl alcohol film. Polarizing plate waste liquid is a by-product produced in the process of manufacturing polarizing plates. Its main components include potassium iodide, boric acid and iodine.
[0003] At present, there are many studies on the treatment methods of boric acid in polarizing plate waste liquid. For example, CN109553116A discloses a method for purifying potassium iodide waste liquid containing boric acid. The method removes boric acid in the form of calcium borate by using calcium hydroxide, but it is not clear how to recover the iodine therein, and how to ensure the purity and yield of the recovered iodine. The existing processes and devices for recovering elemental iodine mainly include: using resin to adsorb iodine and then sublimating and desublimating to obtain industrial crude iodine; or using ethanol and potassium iodide as iodine absorption liquid to absorb iodine vapor generated by sublimation; or using a rolling desublimation barrel to reduce manual operation; or absorbing and concentrating the iodine-containing tail gas generated during the reaction process and then recovering it. However, the above-mentioned method for recovering elemental iodine cannot take into account the purity and recovery rate of iodine, and the waste liquid treatment is insufficient, which is easy to cause resource waste and environmental pollution problems.
[0004] Therefore, providing a comprehensive recycling method for polarizing plate waste liquid so as to maximize resource recycling and ensure the purity and recovery rate of the recycled product is a technical problem that needs to be solved in the current field. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a comprehensive recycling method for polarizer waste liquid. Compared with the prior art, the comprehensive recycling method provided by the present invention can obtain products such as elemental iodine, boric acid, zinc borate and potassium salt, and can maximize the resource utilization of polarizer waste liquid. The obtained products have high purity and recovery rate, and have economic and environmental benefits.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] The present invention provides a comprehensive recycling method for polarizing plate waste liquid, and the comprehensive recycling method comprises the following steps:
[0008] (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid;
[0009] (2) acidifying the concentrated liquid obtained in step (1), then adding an oxidant to carry out a heating reaction, wherein the iodine element generated by the reaction is sublimated by heat and separated from the liquid in the form of iodine vapor, and heating the reaction until the iodine element is completely separated from the liquid to obtain a residual reaction material, and the separated iodine vapor is cooled to condense and sublimate to obtain the iodine element;
[0010] (3) The residual reaction material obtained in step (2) is cooled and solid-liquid separated in sequence to obtain a boric acid product and a boric acid-containing potassium salt solution;
[0011] (4) adding a zinc-containing compound to the boric acid-containing potassium salt solution obtained in step (3) to carry out a first stirring reaction, then adding a seed crystal to carry out a second stirring reaction, and then performing solid-liquid separation to obtain a zinc borate product and a potassium salt solution;
[0012] (5) The potassium salt solution obtained in step (4) is sequentially subjected to distillation concentration, cooling and solid-liquid separation to obtain a potassium salt product.
[0013] The comprehensive recycling method provided by the present invention processes the boric acid, potassium iodide and iodine contained in the polarizing plate waste liquid to prepare products such as iodine, boric acid, zinc borate, potassium salt, etc., so as to maximize the utilization of resources. First, the present invention removes excess water by concentrating the polarizing plate waste liquid, and then sublimates the generated iodine to obtain iodine vapor by acidification and addition of an oxidant, and controls the oxidation under the conditions of heating reaction, and then controls the iodine vapor to cool and condense to obtain iodine. Through the above process, the present invention can effectively improve the purity of iodine and the recovery rate of iodine. Then, in the present invention, the solubility of boric acid is reduced by cooling the remaining reaction materials, so that the boric acid crystallizes and precipitates, and a boric acid product with high purity and recovery rate is obtained. Afterwards, a zinc-containing compound is added to a boric acid-containing potassium salt solution, and a water-insoluble precipitate zinc borate is generated by reacting the zinc-containing compound with boric acid, thereby removing the boric acid, and obtaining a potassium salt solution with high purity, and then the potassium salt solution is concentrated by distillation, cooled and solid-liquid separated to obtain a potassium salt product. In summary, the comprehensive recycling method provided by the present invention can not only prepare a variety of products from polarizing plate waste liquid, but also the obtained products have a high recovery rate and purity, which is conducive to industrial application.
[0014] It should be noted that the anions of the potassium salt described in the present invention are generally determined by the anions in the acid solution. In order to obtain a relatively pure potassium salt product, it is necessary to try to avoid introducing too many impurity ions into the system.
[0015] Preferably, the polarizing plate waste liquid in step (1) contains, by mass percentage, 0.5-5% of boric acid, for example, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; 0.1-1% of potassium iodide, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6 %, 0.7%, 0.8%, 0.9% or 1%, but not limited to the listed values, and other values not listed in the numerical range are equally applicable; 0.01-0.1% of iodine element, for example, can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.1%, but not limited to the listed values, and other values not listed in the numerical range are equally applicable.
[0016] Preferably, the endpoint of the concentration is that the mass percentage of potassium iodide in the concentrated liquid is ≥20%, for example, it can be 20%, 21%, 22%, 23%, 24% or 25%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] Preferably, the acid solution used for the acidification in step (2) includes any one of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid, or a combination of at least two or more thereof.
[0018] Preferably, the pH value of the acidified liquid is 1-2, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] In the present invention, the pH value of the acidified feed solution is preferably controlled within a specific range, which can ensure the oxidation rate and the effectiveness of the oxidant and avoid side reactions.
[0020] Preferably, the oxidizing agent comprises hydrogen peroxide and / or hypochlorous acid.
[0021] Preferably, the amount of the oxidant added is 1-1.4 times the theoretical amount added, for example, it can be 1 time, 1.1 times, 1.2 times, 1.3 times or 1.4 times, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] In the present invention, it is preferred to control the amount of the oxidant added to be a multiple of the theoretical amount, so as to ensure that the iodine ions are fully oxidized to elemental iodine and to ensure the recovery rate of iodine. In the present invention, the theoretical amount of the oxidant added refers to the amount of the oxidant added calculated based on the iodine ions to be oxidized and the chemical reaction equation.
[0023] Preferably, the temperature of the heating reaction in step (2) is 40-65°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C or 65°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] In the present invention, by preferably controlling the temperature of the heating reaction, the iodine element can be sublimated at a faster rate, and less water vapor is generated during the sublimation process.
[0025] Preferably, the cooling temperature in step (2) is ≤20°C, for example, it can be 20°C, 19°C, 18°C, 17°C, 16°C or 15°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the iodine vapor separated in step (2) enters a condenser for cooling.
[0027] Preferably, the iodine element obtained by the condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then subjected to solid-liquid separation to obtain an iodine element product.
[0028] Preferably, part of the un-condensed iodine vapor in the condenser enters the spray tower through the air suction duct of the condenser for absorption and fixation.
[0029] In the present invention, the cooling process is preferably controlled to be carried out in a condenser containing a spray device and an air suction duct. On the one hand, the iodine element obtained by condensation can be flushed out of the condenser by the spray device, thereby separating and obtaining an iodine element product with higher purity; on the other hand, a small amount of un-condensed iodine element tail gas can be effectively treated through the air suction duct and the subsequent spray tower, and the treatment process of iodine vapor can be controlled to be a closed process to avoid causing environmental pollution.
[0030] Preferably, the number of stages of the spray tower is ≥ 1, for example, it can be 1, 2 or 3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the absorption liquid used for the absorption and fixation comprises a mixture of ethanol and potassium iodide.
[0032] In the present invention, the ratio of ethanol to potassium iodide in the absorption liquid can adopt any ratio of ethanol to potassium iodide commonly used in the field for absorbing iodine vapor, for example, it can generally be ethanol and potassium iodide with a mass concentration of 10-20%, prepared in a volume ratio of 1:1.
[0033] Preferably, the terminal temperature of the cooling in step (3) is ≤30°C, for example, it can be 30°C, 29°C, 28°C, 27°C, 26°C, 25°C, 24°C, 23°C, 22°C, 21°C or 20°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the zinc-containing compound in step (4) comprises any one of zinc salt, zinc oxide or zinc hydroxide, or a combination of at least two thereof.
[0035] Preferably, the zinc salt includes any one of zinc sulfate, zinc chloride, zinc nitrate or zinc phosphate, or a combination of at least two thereof.
[0036] Preferably, the zinc-containing compound contains Zn 2+ The ratio of the molar amount of boric acid to the molar amount of boric acid in the boric acid-containing potassium salt solution is (1.4-1.6):1, for example, it can be 1.4:1, 1.42:1, 1.44:1, 1.46:1, 1.48:1, 1.5:1, 1.52:1, 1.54:1, 1.56:1, 1.58:1 or 1.6:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] In the present invention, by preferably controlling the Zn in the zinc-containing compound 2+ The molar amount of zinc in the potassium salt solution is the ratio of the molar amount of boric acid to the molar amount of boric acid in the boric acid-containing potassium salt solution. By adding a sufficient amount of zinc, the boric acid in the potassium salt solution can be completely combined with zinc to form a zinc borate precipitate and thus removed. If too little zinc is added, the boric acid cannot be completely removed. If too much zinc is added, too many zinc ions will be introduced.
[0038] Preferably, the seed crystals comprise zinc borate.
[0039] Preferably, the rotation speed of the first stirring reaction is 50-100 rpm, for example, it can be 50 rpm, 55 rpm, 60 rpm, 65 rpm, 70 rpm, 75 rpm, 80 rpm, 85 rpm, 90 rpm, 95 rpm or 100 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, the first stirring reaction time is 1-5 h, for example, 1 h, 2 h, 3 h, 4 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] In the present invention, the rotation speed and time of the first stirring reaction are preferably controlled within a specific range. Generally, the first stirring reaction adopts a higher rotation speed than the second stirring reaction. The high rotation speed and long stirring time can make the materials fully contact and react so that the boric acid in the materials can completely form zinc borate.
[0042] Preferably, the rotation speed of the second stirring reaction is 20-30 rpm, for example, it can be 20 rpm, 21 rpm, 22 rpm, 23 rpm, 24 rpm, 25 rpm, 26 rpm, 27 rpm, 28 rpm, 29 rpm or 30 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Preferably, the second stirring reaction time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] In the present invention, by preferably controlling the rotation speed and time of the second stirring reaction within a specific range, generally the second stirring reaction adopts a lower rotation speed than the first stirring reaction, and the formed zinc borate can be grown into larger zinc borate particles with the input zinc borate seed crystals as crystal nuclei by reducing the rotation speed, which is convenient for subsequent solid-liquid separation.
[0045] Preferably, the endpoint of the distillation and concentration in step (5) is a solid-liquid ratio ≥ 2:1, for example, it can be 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1 or 3:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] Preferably, the terminal temperature of the cooling in step (5) is ≤30°C, for example, it can be 30°C, 29°C, 28°C, 27°C, 26°C, 24°C or 25°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the solid-liquid separation method includes filtration or centrifugation.
[0048] Wherein, the solid-liquid separation in step (3) may be, for example, centrifugal separation in a centrifugal device, the solid-liquid separation in step (4) may be, for example, filtration separation, and the solid-liquid separation in step (5) may be, for example, centrifugal separation in a centrifugal device. It is further preferred that the solid-liquid separation performed after the iodine elemental product in step (2) is discharged from the condenser may be centrifugal separation in a centrifugal device.
[0049] As a preferred technical solution of the present invention, the comprehensive recycling method comprises the following steps:
[0050] (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid, wherein the mass percentage of potassium iodide in the concentrated feed liquid is ≥ 20%, and the polarizing plate waste liquid contains 0.5-5% of boric acid, 0.1-1% of potassium iodide and 0.01-0.1% of iodine element by mass percentage;
[0051] (2) acidifying the concentrated liquid obtained in step (1), wherein the acid used for the acidification comprises any one of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid or a combination of at least two or more thereof, wherein the pH value of the liquid after acidification is 1-2, then adding an oxidant and performing a heating reaction at a temperature of 40-65° C., wherein the oxidant comprises hydrogen peroxide and / or hypochlorous acid, and the amount of the oxidant added is 1-1.4 times the theoretical amount of the oxidant added, and the iodine element generated by the reaction is heated and sublimated and separated from the liquid in the form of iodine vapor, and the heating reaction is performed until the iodine element is completely separated from the liquid to obtain a residual reaction material, wherein the separated iodine vapor enters a condenser and is cooled and condensed at a temperature of ≤20° C. to obtain iodine element, wherein the iodine element obtained by condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then subjected to solid-liquid separation to obtain an iodine element product, and a portion of the iodine vapor that has not condensed enters a spray tower with a stage number of ≥1 through an air suction duct of the condenser and is absorbed and fixed by a mixed solution of ethanol and potassium iodide;
[0052] (3) The reaction residue obtained in step (2) is cooled to ≤30° C., and then solid-liquid separation is performed to obtain a boric acid product and a boric acid-containing potassium salt solution;
[0053] (4) adding a zinc-containing compound to the boric acid-containing potassium salt solution obtained in step (3), wherein Zn 2+ The ratio of the molar amount of zinc borate to the molar amount of boric acid in the boric acid-containing potassium salt solution is (1.4-1.6): 1, a first stirring reaction is carried out at 50-100 rpm for 1-5 hours, and then zinc borate seeds are added to carry out a second stirring reaction at a rotation speed of 20-30 rpm for 1-3 hours, followed by solid-liquid separation to obtain a zinc borate product and a potassium salt solution, wherein the zinc-containing compound comprises any one of zinc salt, zinc oxide or zinc hydroxide or a combination of at least two thereof, and the zinc salt comprises any one of zinc sulfate, zinc chloride, zinc nitrate or zinc phosphate or a combination of at least two thereof;
[0054] (5) distilling and concentrating the potassium salt solution obtained in step (4) to a solid-liquid ratio of ≥2:1, then cooling to ≤30° C., and then separating the solid and the liquid to obtain a potassium salt product;
[0055] The solid-liquid separation method includes filtration or centrifugation.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] (1) In the comprehensive recycling method provided by the present invention, by controlling the acidification and adding the oxidant, the reaction is carried out under heating conditions, so that the generated iodine element can be sublimated and separated from the feed liquid, and then the iodine vapor is condensed to fix and recover the iodine in the form of iodine element, which can not only effectively improve the purity of the recovered iodine, but also has a higher recovery rate.
[0058] (2) In the comprehensive recycling method provided by the present invention, by adding a zinc-containing compound and zinc borate seed crystals, boric acid and the zinc-containing compound are allowed to generate insoluble zinc borate crystals, which are then removed, thereby obtaining a zinc borate product and a potassium salt solution with a relatively high purity, which is beneficial for the subsequent further preparation of a potassium salt product.
[0059] (3) The comprehensive recycling method provided by the present invention processes the boric acid, potassium iodide and iodine contained in the polarizing plate waste liquid, and can prepare products such as iodine, boric acid, zinc borate, and potassium salt. Under optimal conditions, the purity of iodine can reach more than 99.5%, and the recovery rate of iodine can reach more than 90.5%; the purity of boric acid can reach more than 95.6%, the purity of zinc borate can reach more than 97.9%, and the recovery rate of boric acid can reach more than 99.6%; the purity of potassium salt can reach more than 97.9%, and the recovery rate of potassium can reach more than 93.5%. It can achieve maximum utilization of resources, has economic and environmental benefits, and is conducive to industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a schematic flow chart of the comprehensive recycling method described in Example 1 of the present invention. DETAILED DESCRIPTION
[0061] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0062] Example 1
[0063] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid, such as Figure 1 As shown, the comprehensive recycling method comprises the following steps:
[0064] (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid, wherein the mass percentage of potassium iodide in the concentrated feed liquid is 20%, and the polarizing plate waste liquid contains 5% of boric acid, 0.9% of potassium iodide and 0.01% of iodine by mass percentage;
[0065] (2) the concentrated feed liquid obtained in step (1) is acidified with sulfuric acid, wherein the pH value of the acidified feed liquid is 1.5, and then hydrogen peroxide is added to carry out heating reaction at a temperature of 50° C., wherein the amount of hydrogen peroxide added is 1.2 times the theoretical amount, and the iodine element generated by the reaction is heated and sublimated and separated from the feed liquid in the form of iodine vapor. The heating reaction is carried out until the iodine element is completely separated from the feed liquid to obtain a reaction residual material, and the separated iodine vapor enters a condenser and is cooled and condensed at a temperature of 20° C. to obtain iodine element, and the iodine element obtained by condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then centrifuged to obtain an iodine element product, and part of the iodine vapor that has not condensed enters a three-stage spray tower through an air suction duct of the condenser and is absorbed and fixed by a mixed solution of ethanol and potassium iodide;
[0066] (3) The reaction residue obtained in step (2) is cooled to 30° C. and then centrifuged to obtain a boric acid product and a boric acid-containing potassium salt solution;
[0067] (4) adding zinc oxide to the boric acid-containing potassium salt solution obtained in step (3), wherein Zn 2+ The ratio of the molar amount of zinc borate to the molar amount of boric acid in the boric acid-containing potassium salt solution is 1.5:1, a first stirring reaction is carried out at 70 rpm for 3 hours, and then zinc borate seed crystals are added and a second stirring reaction is carried out at a rotation speed of 25 rpm for 2 hours, and then filtered and separated to obtain a zinc borate product and a potassium salt solution;
[0068] (5) The potassium salt solution obtained in step (4) is distilled and concentrated to a solid-liquid ratio of 2:1, then cooled to 30° C., and then centrifuged to obtain a potassium salt product.
[0069] Example 2
[0070] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid, and the comprehensive recycling method comprises the following steps:
[0071] (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid, wherein the mass percentage of potassium iodide in the concentrated feed liquid is 22%, and the polarizing plate waste liquid contains 2% of boric acid, 0.5% of potassium iodide and 0.1% of iodine by mass percentage;
[0072] (2) the concentrated feed liquid obtained in step (1) is acidified with hydrochloric acid, wherein the pH value of the feed liquid after acidification is 1, and then hypochlorous acid is added and heated to react at a temperature of 40° C., wherein the amount of hypochlorous acid added is 1 times the theoretical amount, and the iodine element generated by the reaction is heated and sublimated and separated from the feed liquid in the form of iodine vapor, and the heating reaction is carried out until the iodine element is completely separated from the feed liquid to obtain a reaction residual material, wherein the separated iodine vapor enters a condenser and is cooled and condensed at a temperature of 19° C. to obtain iodine element, and the iodine element obtained by condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then centrifuged to obtain an iodine element product, and part of the iodine vapor that has not condensed enters a three-stage spray tower through an air suction duct of the condenser and is absorbed and fixed by a mixed solution of ethanol and potassium iodide;
[0073] (3) The reaction residue obtained in step (2) is cooled to 29° C. and then centrifuged to obtain a boric acid product and a boric acid-containing potassium salt solution;
[0074] (4) adding zinc hydroxide to the boric acid-containing potassium salt solution obtained in step (3), wherein the zinc hydroxide contains Zn 2+ The ratio of the molar amount of zinc borate to the molar amount of boric acid in the boric acid-containing potassium salt solution is 1.4:1, a first stirring reaction is carried out at 90 rpm for 1 hour, and then zinc borate seed crystals are added and a second stirring reaction is carried out at a rotation speed of 20 rpm for 3 hours, and then filtered and separated to obtain a zinc borate product and a potassium salt solution;
[0075] (5) The potassium salt solution obtained in step (4) is distilled and concentrated to a solid-liquid ratio of 2.1:1, then cooled to 29° C., and then centrifuged to obtain a potassium salt product.
[0076] Example 3
[0077] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid, and the comprehensive recycling method comprises the following steps:
[0078] (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid, wherein the mass percentage of potassium iodide in the concentrated feed liquid is 21%, and the polarizing plate waste liquid contains 0.5% of boric acid, 0.2% of potassium iodide and 0.05% of iodine by mass percentage;
[0079] (2) the concentrated feed liquid obtained in step (1) is acidified with nitric acid, wherein the pH value of the feed liquid after acidification is 2, and then hydrogen peroxide is added to carry out heating reaction at a temperature of 65° C., wherein the amount of hydrogen peroxide added is 1.4 times the theoretical amount, and the iodine element generated by the reaction is heated and sublimated and separated from the feed liquid in the form of iodine vapor. The heating reaction is carried out until the iodine element is completely separated from the feed liquid to obtain a reaction residual material, wherein the separated iodine vapor enters a condenser and is cooled and condensed at a temperature of 18° C. to obtain iodine element, and the iodine element obtained by condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then centrifuged to obtain an iodine element product, and part of the iodine vapor that has not condensed enters a three-stage spray tower through an air suction duct of the condenser and is absorbed and fixed by a mixed solution of ethanol and potassium iodide;
[0080] (3) The reaction residue obtained in step (2) is cooled to 28° C. and then centrifuged to obtain a boric acid product and a boric acid-containing potassium salt solution;
[0081] (4) adding zinc nitrate to the boric acid-containing potassium salt solution obtained in step (3), wherein Zn 2+ The ratio of the molar amount of zinc borate to the molar amount of boric acid in the boric acid-containing potassium salt solution is 1.6:1, a first stirring reaction is carried out at 50 rpm for 5 hours, and then zinc borate seed crystals are added and a second stirring reaction is carried out at a rotation speed of 30 rpm for 1 hour, and then filtered and separated to obtain a zinc borate product and a potassium salt solution;
[0082] (5) The potassium salt solution obtained in step (4) is distilled and concentrated to a solid-liquid ratio of 2.2:1, then cooled to 28° C., and then centrifuged to obtain a potassium salt product.
[0083] Example 4
[0084] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The only difference between the comprehensive recycling method and Embodiment 1 is that the heating reaction temperature is 37°C.
[0085] Example 5
[0086] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The only difference between the comprehensive recycling method and Embodiment 1 is that the heating reaction temperature is 70°C.
[0087] Example 6
[0088] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The difference between the comprehensive recycling method and embodiment 1 is that the Zn in zinc oxide is 2+ The ratio of the molar amount of boric acid to the molar amount of boric acid in the boric acid-containing potassium salt solution is 0.8:1.
[0089] Example 7
[0090] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The difference between the comprehensive recycling method and embodiment 1 is that the Zn in zinc oxide is 2+ The ratio of the molar amount of boric acid to the molar amount of boric acid in the boric acid-containing potassium salt solution is 2.2:1.
[0091] Example 8
[0092] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The difference between the comprehensive recycling method and Embodiment 1 is that the rotation speed of the first stirring reaction is 20 rpm.
[0093] Example 9
[0094] This embodiment provides a comprehensive recycling method for polarizing plate waste liquid. The difference between the comprehensive recycling method and Embodiment 1 is that the rotation speed of the second stirring reaction is 70 rpm.
[0095] Comparative Example 1
[0096] This comparative example provides a method for treating polarizing plate waste liquid, the method comprising:
[0097] (1) The polarizing plate waste liquid (same as in Example 1) is concentrated to a mass percentage of potassium iodide of 20%, and then sulfuric acid is added to acidify to a pH value of 4, and then filtered to separate to obtain boric acid and an iodine-containing solution;
[0098] (2) adding sulfuric acid to the iodine-containing solution obtained in step (1) for secondary acidification until the pH value is 1.5, adding 1.2 times the theoretical amount of sodium perborate as an oxidant, and controlling the oxidation temperature to be below 25° C. to obtain a solid-liquid mixture containing elemental iodine and boric acid;
[0099] (3) adding potassium hydroxide to the solid-liquid mixture obtained in step (2) to adjust the pH value to 7, and then filtering to obtain iodine and potassium salt solution;
[0100] (4) The potassium salt solution of step (3) is distilled and concentrated to a solid-liquid ratio of 2:1, then cooled to 30° C., and then centrifuged to obtain a potassium salt product.
[0101] Comparative Example 2
[0102] This comparative example provides a method for treating polarizing plate waste liquid. The difference between the treatment method and Example 1 is that step (4) is not performed, and the boric acid-containing potassium salt solution obtained in step (3) is directly subjected to distillation concentration, cooling and centrifugal separation in step (5) to obtain a potassium salt product.
[0103] The purity of the products obtained in Examples 1-9 and Comparative Examples 1-2 was tested, wherein the detection of iodine element was carried out according to GBZ / T 300.58-2017, the detection of boric acid was carried out according to GB 5009.275-2016, the detection of zinc borate was carried out according to Q / ZXB003-2009, and the detection of potassium sulfate was carried out according to GB / T 10725-2015. The results are shown in Table 1.
[0104] The recovery rates of the products obtained in Examples 1-9 and Comparative Examples 1-2 were tested, and the results are shown in Table 1, wherein the iodine recovery rate was calculated as follows: the mass of recovered iodine / the mass of all iodine elements in the polarizing plate waste liquid × 100%; the boric acid recovery rate was calculated as follows: the sum of the masses of the recovered boric acid and the boric acid corresponding to zinc borate / the mass of boric acid in the polarizing plate waste liquid × 100%; and the potassium recovery rate was calculated as follows: the mass of potassium in potassium salt / the mass of potassium in the polarizing plate waste liquid × 100%.
[0105] Table 1
[0106]
[0107]
[0108] In Table 1, “ / ” means that the data is not available.
[0109] From the data in Table 1, we can see the following points:
[0110] (1) It can be seen from the data of Examples 1-3 that, under optimal conditions, the comprehensive recovery and utilization method provided by the present invention can make the purity of elemental iodine reach more than 99.5%, and the recovery rate of iodine reach more than 90.5%; the purity of boric acid can reach more than 95.6%, the purity of zinc borate can reach more than 97.9%, and the recovery rate of boric acid can reach more than 99.6%; the purity of potassium salt can reach more than 97.9%, and the recovery rate of potassium can reach more than 93.5%.
[0111] (2) A comprehensive comparison of the data of Example 1 and Examples 4-5 shows that the only difference between Example 4-5 and Example 1 is that the temperature of the heating reaction is not within the preferred range of the present invention. The iodine recovery rate in Example 1 is significantly higher than that in Examples 4-5. It can be seen that the present invention can further promote the sublimation of iodine and improve the iodine recovery rate by preferably controlling the temperature of the heating reaction.
[0112] (3) Comprehensive comparison of the data of Example 1 and Examples 6-7 shows that the difference between Example 6-7 and Example 1 is only that Zn in zinc oxide 2+The molar amount of Zn in zinc oxide is not within the preferred range of the present invention. The recovery rate of boric acid in Example 6 is significantly lower than that in Example 1. The purity of potassium salt in Example 7 is significantly lower than that in Example 1. It can be seen that the present invention can achieve the desired effect by preferably controlling the molar amount of Zn in zinc oxide. 2+ The ratio of the molar amount of zinc ions to the molar amount of boric acid in the boric acid-containing potassium salt solution can improve the boric acid recovery rate while avoiding the introduction of excessive zinc ions, thereby ensuring the purity of the potassium salt.
[0113] (4) Comprehensive comparison of the data of Example 1 and Examples 8-9 shows that the only difference between Example 8-9 and Example 1 is that the rotation speed of the first stirring reaction and the rotation speed of the second stirring reaction are not within the preferred range of the present invention, respectively. The recovery rate of boric acid in Example 8-9 is significantly lower than that in Example 1, and the purity of the potassium salt is significantly lower than that in Example 1. It can be seen that the present invention can further promote the complete conversion of boric acid into zinc borate, improve the recovery rate of boric acid, promote solid-liquid separation, and ensure the purity of the potassium salt by preferably controlling the rotation speeds of the first stirring reaction and the second stirring reaction within a specific range.
[0114] (5) Comprehensive comparison of the data of Example 1 and Comparative Examples 1-2 shows that in Comparative Example 1, the oxidation reaction is not controlled to be carried out under heating conditions, so that the generated iodine element is still retained in the solution, and high-purity and high-recovery iodine element cannot be obtained. In addition, the purity of boric acid and potassium salt in Example 1 is also significantly higher than that in Comparative Example 1. In Comparative Example 2, no zinc-containing compound is added to treat the boric acid contained in the potassium salt solution. The purity, recovery rate of boric acid and purity of potassium salt in Example 1 are significantly higher than those in Comparative Example 2. It can be seen that the comprehensive recycling method provided by the present invention can improve the purity and recovery rate of the product.
[0115] In summary, the comprehensive recycling method provided by the present invention can obtain products such as elemental iodine, boric acid, zinc borate and potassium salt, which can maximize the resource utilization of polarizing plate waste liquid, and the obtained products have high purity and recovery rate, and have economic and environmental benefits.
[0116] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A comprehensive recycling method for polarizing plate waste liquid, characterized in that: The comprehensive recycling method comprises the following steps: (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid; (2) acidifying the concentrated liquid obtained in step (1), then adding an oxidant to carry out a heating reaction, wherein the iodine element generated by the reaction is sublimated by heat and separated from the liquid in the form of iodine vapor, and heating the reaction until the iodine element is completely separated from the liquid to obtain a residual reaction material, and the separated iodine vapor is cooled to condense and sublimate to obtain the iodine element; (3) The residual reaction material obtained in step (2) is cooled and solid-liquid separated in sequence to obtain a boric acid product and a boric acid-containing potassium salt solution; (4) adding a zinc-containing compound to the boric acid-containing potassium salt solution obtained in step (3) to carry out a first stirring reaction, then adding a seed crystal to carry out a second stirring reaction, and then performing solid-liquid separation to obtain a zinc borate product and a potassium salt solution; (5) The potassium salt solution obtained in step (4) is sequentially subjected to distillation concentration, cooling and solid-liquid separation to obtain a potassium salt product.
2. The comprehensive recycling method according to claim 1, characterized in that: The polarizing plate waste liquid in step (1) contains, by weight percentage, 0.5-5% of boric acid, 0.1-1% of potassium iodide and 0.01-0.1% of elemental iodine; Preferably, the end point of the concentration is that the mass percentage of potassium iodide in the concentrated liquid is ≥ 20%.
3. The comprehensive recycling method according to claim 1 or 2, characterized in that: The acid used in the acidification in step (2) includes any one of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid, or a combination of at least two or more thereof; Preferably, the pH value of the acidified liquid is 1-2; Preferably, the oxidant comprises hydrogen peroxide and / or hypochlorous acid; Preferably, the amount of the oxidant added is 1-1.4 times the theoretical amount.
4. The comprehensive recycling method according to any one of claims 1 to 3, characterized in that: The temperature of the heating reaction in step (2) is 40-65°C; Preferably, the cooling temperature in step (2) is ≤20°C.
5. The comprehensive recycling method according to any one of claims 1 to 4, characterized in that: The iodine vapor separated in step (2) enters a condenser for cooling; Preferably, the iodine element obtained by the desublimation is sprayed by a spray device in the condenser and then discharged from the condenser, and then subjected to solid-liquid separation to obtain an iodine element product; Preferably, part of the un-condensed iodine vapor in the condenser enters the spray tower through the air suction pipe of the condenser for absorption and fixation; Preferably, the number of stages of the spray tower is ≥1; Preferably, the absorption liquid used for the absorption and fixation comprises a mixture of ethanol and potassium iodide.
6. The comprehensive recycling method according to any one of claims 1 to 5, characterized in that: The cooling end point temperature in step (3) is ≤30°C.
7. The comprehensive recycling method according to any one of claims 1 to 6, characterized in that: The zinc-containing compound in step (4) includes any one of zinc salt, zinc oxide or zinc hydroxide, or a combination of at least two thereof; Preferably, the zinc salt comprises any one or a combination of at least two of zinc sulfate, zinc chloride, zinc nitrate or zinc phosphate; Preferably, the zinc-containing compound contains Zn 2+ The ratio of the molar amount of boric acid to the molar amount of boric acid in the boric acid-containing potassium salt solution is (1.4-1.6):1; Preferably, the seed crystals include zinc borate; Preferably, the rotation speed of the first stirring reaction is 50-100 rpm; Preferably, the first stirring reaction time is 1-5h; Preferably, the rotation speed of the second stirring reaction is 20-30 rpm; Preferably, the second stirring reaction time is 1-3 hours.
8. The comprehensive recycling method according to any one of claims 1 to 7, characterized in that: The end point of the distillation concentration in step (5) is a solid-liquid ratio ≥ 2:1; Preferably, the terminal temperature of the cooling in step (5) is ≤30°C.
9. The comprehensive recycling method according to any one of claims 1 to 8, characterized in that: The solid-liquid separation method includes filtration or centrifugation.
10. The comprehensive recycling method according to any one of claims 1 to 9, characterized in that: The comprehensive recycling method comprises the following steps: (1) concentrating the polarizing plate waste liquid to obtain a concentrated feed liquid, wherein the mass percentage of potassium iodide in the concentrated feed liquid is ≥ 20%, and the polarizing plate waste liquid contains 0.5-5% of boric acid, 0.1-1% of potassium iodide and 0.01-0.1% of iodine element by mass percentage; (2) acidifying the concentrated liquid obtained in step (1), wherein the acid used for the acidification comprises any one of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid or a combination of at least two or more thereof, wherein the pH value of the liquid after acidification is 1-2, then adding an oxidant and performing a heating reaction at a temperature of 40-65° C., wherein the oxidant comprises hydrogen peroxide and / or hypochlorous acid, and the amount of the oxidant added is 1-1.4 times the theoretical amount of the oxidant added, and the iodine element generated by the reaction is heated and sublimated and separated from the liquid in the form of iodine vapor, and the heating reaction is performed until the iodine element is completely separated from the liquid to obtain a residual reaction material, wherein the separated iodine vapor enters a condenser and is cooled and condensed at a temperature of ≤20° C. to obtain iodine element, wherein the iodine element obtained by condensation is sprayed by a spray device in the condenser and then discharged from the condenser, and then subjected to solid-liquid separation to obtain an iodine element product, and a portion of the iodine vapor that has not condensed enters a spray tower with a stage number of ≥1 through an air suction duct of the condenser and is absorbed and fixed by a mixed solution of ethanol and potassium iodide; (3) The reaction residue obtained in step (2) is cooled to ≤30° C., and then solid-liquid separation is performed to obtain a boric acid product and a boric acid-containing potassium salt solution; (4) adding a zinc-containing compound to the boric acid-containing potassium salt solution obtained in step (3), wherein Zn 2 + The ratio of the molar amount of zinc borate to the molar amount of boric acid in the boric acid-containing potassium salt solution is (1.4-1.6): 1, a first stirring reaction is carried out at 50-100 rpm for 1-5 hours, and then zinc borate seeds are added to carry out a second stirring reaction at a rotation speed of 20-30 rpm for 1-3 hours, followed by solid-liquid separation to obtain a zinc borate product and a potassium salt solution, wherein the zinc-containing compound comprises any one of zinc salt, zinc oxide or zinc hydroxide or a combination of at least two thereof, and the zinc salt comprises any one of zinc sulfate, zinc chloride, zinc nitrate or zinc phosphate or a combination of at least two thereof; (5) distilling and concentrating the potassium salt solution obtained in step (4) to a solid-liquid ratio of ≥2:1, then cooling to ≤30° C., and then separating the solid and the liquid to obtain a potassium salt product; The solid-liquid separation method includes filtration or centrifugation.
Citation Information
Patent Citations
Method for recovering elemental iodine and boric acid from iodine-containing waste liquid
CN116902990A
Method for recovering iodine from waste fluid in polarizing film production