Preparation method and application of low-ash biomass carbon precursor material

Through the combined use of acids, hydrogen fluoride and oxidizer, the problems of high ash content and long preparation time of biomass carbon precursor materials in the hydrothermal method are solved, and low ash hard carbon materials are prepared, suitable for the negative electrode of sodium ion batteries, improving the material stability and marketing value.

CN118929630APending Publication Date: 2024-11-12HUZHOU YICHAN NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411121001.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the existing hydrothermal method prepares biomass carbon precursor materials, the ash content is high, the preparation time is long, the autocatalytic process is difficult to start and the silicon-containing components are difficult to completely remove, which limits its application in the fields of new energy and power electronics.

Method used

The combination of acid additive A, hydrogen fluoride or fluorine-containing salt compound additive B and oxidant additive C is used to regulate the hydrothermal reaction temperature and time, promote the depolymerization and dehydration of biomass macromolecules, reduce the ash content, and The preparation of low-ash carbon precursor material is achieved by combining additive A with metal ions and removing silicon by additive B.

Benefits of technology

The preparation of low-ash carbon precursor materials has been realized. The product forms low-ash hard carbon materials after high-temperature pyrolysis, with stable sodium storage capacity, suitable for multiple charge and discharge cycles, and is compatible with a variety of cheap biomass raw materials, reducing the Production cost and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995086280000061
    Figure BDA0004995086280000061
  • Figure BDA0004995086280000071
    Figure BDA0004995086280000071
  • Figure HDA0004995086290000011
    Figure HDA0004995086290000011
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy materials, and relates to a preparation method and application of a low-ash biomass carbon precursor material. The preparation method comprises the following steps: S1, proportioning a biomass raw material and water to obtain slurry; s2, adding an auxiliary agent A, an auxiliary agent B and an auxiliary agent C into the slurry, uniformly mixing, carrying out hydrothermal reaction, setting the hydrothermal reaction temperature to be 120-300 DEG C, and keeping the temperature for 1-240 minutes, so as to obtain reacted slurry; the aid A is an acid or acid-containing solution which provides anions with metal combined in the biomass; the auxiliary agent B is hydrogen fluoride or a fluorine-containing salt compound; the auxiliary C is an oxidizing agent; s3, carrying out solid-liquid separation on the reacted slurry to obtain a solid crude product; and S4, washing, drying and crushing the solid crude product to form the low-ash biomass carbon precursor material. According to the invention, a low-ash-content carbon precursor product can be prepared, and a hard carbon material prepared from the low-ash-content carbon precursor product can maintain relatively stable sodium storage capacity under multiple charge-discharge cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy materials, and in particular relates to a preparation method of a low-ash biomass carbon precursor material and an application thereof. Background Art

[0002] The hydrothermal method is a green and gentle method for producing biomass carbon materials. Biomass raw materials can be taken from agricultural and forestry industry waste, and the reaction temperature is generally not higher than 300°C, with low production costs. In a hydrothermal environment, the high molecular substances in the biomass undergo a process of "depolymerization-aromatization-repolymerization" to form carbon-rich precursor materials. During this process, the high molecular weight substances will also undergo decarboxylation reactions to form small molecular organic acids. These organic acids can act as catalysts to promote the decomposition of biomass macromolecules and the dehydration of small molecules. On the other hand, they can also combine with the metal ions exposed in the raw materials and dissolve in the reaction solution together to achieve deashing of the product.

[0003] In a hydrothermal environment, the depolymerization, decarboxylation and dehydration reactions of macromolecules in biomass and small molecules can be spontaneously completed, but at a lower temperature, this series of reactions occurs slowly, the autocatalytic process is difficult to start, the time required to prepare biomass carbon precursors is long, and the spontaneously generated organic acid cannot be adjusted to bind metal ions, the degree of deashing and impurity removal is limited, and many biomasses contain silicon-containing components, which cannot be removed by hydrothermal treatment in general, and require special silicon removal treatment. Patents CN111439738B and CN106744798B add impregnation and silicon removal steps before and after biomass carbonization, respectively, which takes a long time to prepare the material and is costly. After carbonization, part of the silicon-containing material is wrapped inside the carbon particles, which is difficult to completely remove by impregnation, and the removal effect of silicon is limited. The lignin part in the biomass can only be partially dissolved in the reaction solvent during the hydrothermal reaction, resulting in the metal ions bound thereto being difficult to effectively remove. In addition, the hydrothermal treatment time in the prior art is relatively long, generally up to several hours. In summary, the existing technologies generally have problems such as high ash content in the prepared carbon precursor materials, difficulty in further reducing the ash content in the product, and a long hydrothermal process, which limits the application of hydrothermal carbon materials in the fields of new energy and power electronics. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a low-ash biomass carbon precursor material in view of the deficiencies of the prior art. The preparation method provided by the present invention can prepare a low-ash carbon precursor product, and the low-ash carbon precursor is pyrolyzed at high temperature to obtain a low-ash hard carbon material, which can maintain a relatively stable sodium storage capacity under multiple charge and discharge cycles.

[0005] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:

[0006] A method for preparing a low-ash biomass carbon precursor material comprises the following steps:

[0007] S1 uses biomass raw materials and water to prepare slurry;

[0008] Adding additives A, B and C to the S2 slurry, mixing evenly and performing a hydrothermal reaction, the hydrothermal reaction temperature is set to 120-300°C, and the temperature is kept for 1-240 minutes to obtain a slurry after the reaction; the additive A is an acid or an acid-containing solution that provides anions that bind to metals in biomass, and the specific selection of the acid includes inorganic acids, organic acids or acid salts, etc.; the additive B is hydrogen fluoride or a fluoride salt compound; the additive C is an oxidant;

[0009] S3: performing solid-liquid separation on the slurry after the reaction to obtain a solid crude product;

[0010] S4 washes, dries and crushes the solid crude product to form a low-ash biomass carbon precursor material. According to the above scheme, the fluoride salt compound in the auxiliary agent B includes one or more of ammonium fluoride, sodium fluoride, potassium fluoride and hydrofluoric acid.

[0011] According to the above scheme, the auxiliary agent A is selected from one or more of polyphosphoric acid, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium hydrogen phosphite, ethylenediaminetetraacetic acid, acrylic acid, methacrylic acid, citric acid and tartaric acid, or a combination thereof with an inorganic acid, preferably one or more of ethylenediaminetetraacetic acid, acrylic acid, methacrylic acid and tartaric acid, or a combination thereof with an inorganic acid.

[0012] According to the above scheme, the auxiliary agent C oxidant is selected from one or a combination of hydrogen peroxide, sodium peroxide, ammonium persulfate, sodium hypochlorite, and sodium perchlorate.

[0013] According to the above scheme, the auxiliary agent A is one or more of ethylenediaminetetraacetic acid, acrylic acid, methacrylic acid, citric acid and tartaric acid, or a combination thereof with an inorganic acid; the auxiliary agent C is one or more of hydrogen peroxide, sodium peroxide and ammonium persulfate.

[0014] According to the above scheme, the amount of auxiliary agent A added in step S2 is 0.1-5wt% of the biomass raw material in S1, the amount of auxiliary agent B added is 0.1-1wt% of the biomass raw material in S1, and the amount of auxiliary agent C added is 0.5-5wt% of the biomass raw material in S1.

[0015] According to the above scheme, the biomass raw material is selected from one or a combination of starch, walnut shells, peach pits, bamboo powder, wood powder, bagasse, straw and rice husk.

[0016] According to the above scheme, the hydrothermal reaction temperature in the S2 step is 160-280°C, and the insulation time is 5-180 min, further 5-120 min, and further, can be 5-90 min.

[0017] According to the above scheme, the mass ratio of biomass raw material to water in step S1 is 1:1-20.

[0018] Preferably, in step S1, the mass ratio of biomass raw material to water is 1:4-10.

[0019] According to the above scheme, the ash content of the biomass carbon precursor material prepared by the above method is not higher than 1%, generally not higher than 0.5%, further, not higher than 0.2%, and more preferably, not higher than 0.1%.

[0020] According to the above scheme, the auxiliary agent A is ethylenediaminetetraacetic acid, the auxiliary agent B is ammonium fluoride or hydrogen fluoride, and the auxiliary agent C is ammonium persulfate. The above auxiliary agents can provide both ammonium ions and anions that can be complexed with metals in the mixed solution provided by the use of the above auxiliary agents. In the closed hydrothermal system, based on the biomass autocatalytic cycle catalyzed by the auxiliary agent A, the removal of silicon by the auxiliary agent B, and the effect of the auxiliary agent C make the biomass macromolecule degradation more thorough, so that the insoluble macromolecules are more converted into soluble small molecules, and then polycondensed into carbon, fully exposing the ash substances in the biomass structure including metal elements and silicon, so that the auxiliary agents A and B are more easily exposed to the ash elements, and the anions provided by the above auxiliary agent A that can bind to the metal in the biomass form soluble complexes or chelates with the metals during the hydrothermal process, remove the metals, and the catalysis of the ammonium ions provided by the auxiliary agent promotes the combination of aromatic molecules and carbon-rich species in the early stage of the hydrothermal reaction, and accelerates the reaction speed, so as to further reduce the hydrothermal reaction time and prepare low-moisture precursor materials. By adjusting the reaction time and the reaction temperature, the ash content of the biomass carbon precursor material prepared from different biomass raw materials is not higher than 0.2%, further, not higher than 0.1%. Even more, not higher than 0.05%. Specifically, the hydrothermal reaction time can be 5-120min, further 5-90min, and further 5-60min, and the hydrothermal reaction temperature is preferably 200-270°C. The ash content of the biomass carbon precursor material prepared by the above method is not higher than 0.2%, more preferably, not higher than 0.1%. Even more, not higher than 0.05%.

[0021] According to the above scheme, in the step S3, the solid-liquid separation of the slurry after the reaction is carried out by centrifugation. The specific steps are: the slurry after the reaction is introduced into a centrifuge, and the solid phase and the liquid phase are separated after high-speed centrifugation, wherein the solid phase is the crude product and the liquid phase is the mother liquor. The crude product is washed with water and ethanol to remove the mother liquor remaining on the surface, and then dried and crushed to obtain a low-ash biomass carbon precursor material. The drying and crushing methods of the product include one or a combination of hot air drying, vacuum drying, freeze drying, grinding and crushing, air flow crushing and ultrasonic crushing.

[0022] The present invention also provides a method for preparing a low-ash hard carbon material, wherein the prepared low-ash biomass carbon precursor material is subjected to high-temperature treatment in an inert atmosphere to form the low-ash hard carbon material.

[0023] According to the above scheme, the high temperature treatment is firstly low temperature pre-carbonization at 400-750°C, and then heating to 1000-1300°C for high temperature treatment to form a low ash hard carbon material.

[0024] The present invention further provides a low-ash hard carbon material obtained by the above preparation method.

[0025] Furthermore, the present invention also provides a sodium ion battery made from the aforementioned low-ash hard carbon material.

[0026] Furthermore, the present invention also provides the use of low-ash hard carbon materials as negative electrode materials for sodium ion batteries.

[0027] The invention uses three auxiliary agents, namely, an acid auxiliary agent A, a hydrogen fluoride or fluorine-containing salt compound auxiliary agent B and an oxidant auxiliary agent C, in combination for the hydrothermal reaction of biomass. The auxiliary agent A reduces the pH value of the initial solution, provides a large amount of hydrogen ions as a catalyst, accelerates the decomposition of biomass macromolecules and the process of forming small molecular acids by side chain decarboxylation, starts the biomass autocatalytic cycle, and shortens the hydrothermal reaction time of the biomass. Furthermore, some anions provided in the auxiliary agent A that can bind to metals in the biomass can also form soluble complexes or chelates with the metals during the hydrothermal process, so that the metal ions are separated from the solid product. The fluorine ions provided by the auxiliary agent B are combined with silicon species in the biomass in an acidic environment, and the auxiliary agent C is used to make the biomass macromolecules degrade more thoroughly, so that the insoluble macromolecules are more converted into soluble small molecules, and then polycondensed into carbon. This process is conducive to fully exposing ash substances in the biomass structure, including metal elements and silicon, so that the auxiliary agents A and B are more easily in contact with the ash elements, and the effects of fully removing silicon and metals that cannot be achieved in the prior art are achieved, so that the ash removal is more thorough. Relatively speaking, the invention has a small amount of auxiliary agent and a short hydrothermal reaction time, which can be as short as a few minutes, and is more economical in production.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention provides a method for preparing a low-ash biomass carbon precursor material. The method can prepare a low-ash carbon precursor product by using three additives, namely, an additive A, a hydrogen fluoride or fluorine-containing salt compound additive B, and an oxidant additive C. The low-ash carbon precursor is subjected to high-temperature pyrolysis to obtain a low-ash hard carbon material, which can maintain a relatively stable sodium storage capacity under multiple charge and discharge cycles.

[0030] (2) The present invention provides a method for preparing a low-ash biomass carbon precursor material, which uses three additives, additive A, hydrogen fluoride or fluorine-containing salt compound additive B, and oxidant additive C, in combination. The amount of additives used is small, and the hydrothermal time is short, so that the prepared carbon precursor material has a low ash content.

[0031] (3) The preparation method provided by the present invention is compatible with a variety of cheap biomass raw materials such as sugars, fruit shells and wood powder, and has high market promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The first cycle charge and discharge curve of the low-ash hard carbon material AC prepared in the embodiment of the present invention;

[0033] Figure 2 This is the cycle curve of the low-ash hard carbon material AC prepared in the embodiment of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention will be fully and clearly described below in conjunction with specific embodiments, but the described embodiments are only some embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] In this embodiment, walnut shells are used as raw materials to prepare low-ash biomass carbon precursor materials, and the specific steps are as follows:

[0037] Walnut shells, ethylenediaminetetraacetic acid, ammonium fluoride, ammonium persulfate and water were added to the reactor in a mass ratio of 100:2:0.3:2:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 220 degrees and hydrothermally reacted for 30 minutes. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product A.

[0038] Example 2

[0039] In this embodiment, walnut shells are used as raw materials to prepare low-ash biomass carbon precursor materials, and the specific steps are as follows:

[0040] Walnut shells, ethylenediaminetetraacetic acid, ammonium fluoride, ammonium persulfate and water were added to the reactor in a mass ratio of 100:2:0.3:2:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 220 degrees and hydrothermally reacted for 5 minutes. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product B.

[0041] Example 3

[0042] In this embodiment, walnut shells are used as raw materials to prepare low-ash biomass carbon precursor materials, and the specific steps are as follows:

[0043] Walnut shells, ethylenediaminetetraacetic acid, ammonium fluoride, ammonium persulfate and water were added to the reactor in a mass ratio of 100:2:0.3:2:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 160 degrees and hydrothermally reacted for 30 minutes. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product B.

[0044] Example 4

[0045] In this embodiment, walnut shells are used as low-ash biomass carbon precursor materials, and the specific steps are as follows:

[0046] Walnut shells, polyphosphoric acid, ammonium fluoride, ammonium persulfate and water were added to the reactor in a mass ratio of 100:0.3:0.3:2:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 220 degrees and hydrothermally reacted for 1 hour. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product D.

[0047] Example 5

[0048] In this embodiment, walnut shells are used as low-ash biomass carbon precursor materials, and the specific steps are as follows:

[0049] Walnut shells, acrylic acid, hydrofluoric acid, hydrogen peroxide and water were added to the reactor in a mass ratio of 100:5:0.3:3:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 220 degrees and subjected to hydrothermal reaction for 2 hours. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product E.

[0050] Example 6

[0051] In this embodiment, bagasse is used as raw material to prepare a low-ash biomass carbon precursor material, and the specific steps are as follows:

[0052] Add bagasse, ethylenediaminetetraacetic acid, potassium fluoride, ammonium persulfate and water to the reactor in a mass ratio of 100:1:0.8:0.5:500, and stir at room temperature for 20 minutes until the slurry is evenly dispersed. Heat the slurry to 200 degrees and hydrothermally react for 10 minutes. After the reaction, place the slurry in a centrifuge and centrifuge at 1500r / min to obtain a solid phase crude product. Wash the crude product with water and ethanol, dry it with hot air and crush it with a ball mill to obtain a finished carbon precursor powder, which is recorded as product F.

[0053] Example 7

[0054] In this embodiment, bagasse is used as raw material to prepare a low-ash biomass carbon precursor material, and the specific steps are as follows:

[0055] Add bagasse, ethylenediaminetetraacetic acid, potassium fluoride, ammonium persulfate and water to the reactor in a mass ratio of 100:1:0.8:0.5:500, and stir at room temperature for 20 minutes until the slurry is evenly dispersed. Heat the slurry to 200 degrees and hydrothermally react for 90 minutes. After the reaction, place the slurry in a centrifuge and centrifuge at 1500r / min to obtain a solid phase crude product. Wash the crude product with water and ethanol, dry it with hot air and crush it with a ball mill to obtain a finished carbon precursor powder, which is recorded as product G.

[0056] Example 8

[0057] In this embodiment, bamboo powder is used as a raw material to prepare a low-ash biomass carbon precursor material, and the specific steps are as follows:

[0058] Bamboo powder, citric acid, ammonium fluoride, ammonium persulfate and water were added to the reactor in a mass ratio of 100:4:0.1:5:500, and stirred at room temperature for 20 minutes until the slurry was evenly dispersed. The slurry was heated to 240 degrees and hydrothermally reacted for 3 hours. After the reaction, the slurry was placed in a centrifuge and centrifuged at 1500r / min to obtain a solid phase crude product. The crude product was washed with water and ethanol, and the carbon precursor powder was obtained after hot air drying and ball mill crushing, which was recorded as product H.

[0059] Example 9

[0060] The low-ash hard carbon material obtained by carbonizing the low-ash biomass carbon precursor material can be used as the negative electrode active material of the sodium ion battery. The specific steps are as follows:

[0061] Product A was heated to 600°C at a rate of 5°C / min under an argon atmosphere, kept at this temperature for 2 hours, then heated to 1300°C at a rate of 2°C / min, kept at this temperature for 2 hours, and then cooled naturally to obtain a low-ash hard carbon material AC.

[0062] The low-ash hard carbon material AC, conductive carbon black and binder are coated on aluminum foil in a ratio of 8:1:1 to form a pole piece, which is used as the pole of the battery with sodium metal. The two are separated by a polypropylene diaphragm, and the electrolyte is added to assemble a button battery. The test shows that the reversible specific capacity of the carbon material is 311mAh / g, and the capacity retention rate is as high as 98% after 100 cycles at a current density of 20mA / g.

[0063] Comparative Example 1

[0064] Walnut shells and water were added to the reactor in a mass ratio of 100:500, without adding an auxiliary agent, and the remaining operations were the same as those in Example 1. The obtained carbon precursor powder product was recorded as comparative product A-.

[0065] Comparative Example 2

[0066] Sugarcane bagasse and water were added to the reactor in a mass ratio of 100:500, without adding an auxiliary agent, and the remaining operations were the same as those in Example 6. The obtained carbon precursor powder product was recorded as comparative product D-.

[0067] Comparative Example 3

[0068] Bamboo powder and water were added to the reactor in a mass ratio of 100:500 without adding an auxiliary agent. The remaining operations were the same as those in Example 8. The obtained carbon precursor powder product was recorded as comparative product H-.

[0069] The key preparation conditions and ash contents of products AH prepared in Examples 1-8 of the present invention and comparative products A-, D-, and E- prepared in Comparative Examples 1-3 are shown in Table 1.

[0070] Table 1

[0071]

[0072]

[0073] The present invention uses three additives, namely, acid additive A, hydrogen fluoride or fluorine-containing salt compound additive B and oxidant additive C, in combination for the hydrothermal reaction of biomass. Through the synergy of these three additives, the ash in the biomass can be effectively removed at a low dosage of additives and a short reaction time, and the ash content of the obtained biomass carbon precursor material is not higher than 0.2%, preferably, not higher than 0.1%, and the lowest can reach 0.03%. It can be seen from Examples 1-5 in Table 1 that the combined use of the three additives A, B, and C in the present invention is effective for a variety of biomass raw materials, among which the combination of ethylenediaminetetraacetic acid, ammonium fluoride and ammonium persulfate has the best effect. The reason may be that ethylenediaminetetraacetic acid has a strong chelating ability for metal ions such as calcium and magnesium, which can effectively remove metal ions, and ammonium persulfate has a slightly higher stability and can be decomposed at a higher temperature. The strong oxidizing species produced can promote the degradation of biomass macromolecules, especially lignin, and can more effectively destroy the original structure of biomass and increase the exposure of ash. The ammonium ions in the additive can also promote the combination of aromatic molecules and carbon-rich species in the early stage of the hydrothermal reaction and accelerate the reaction rate.

[0074] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes that fall within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0075] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a low-ash biomass carbon precursor material, characterized in that: The following steps are involved: S1 uses biomass raw materials and water to prepare slurry; Adding additives A, B and C to the S2 slurry, mixing evenly and performing a hydrothermal reaction, the hydrothermal reaction temperature is set to 120-300°C, and the temperature is kept for 1-240 minutes to obtain a slurry after the reaction; the additive A is an acid or an acid-containing solution that provides anions that can bind metals in biomass; the additive B is hydrogen fluoride or a fluoride salt compound; the additive C is an oxidant; S3: performing solid-liquid separation on the slurry after the reaction to obtain a solid crude product; S4 washes, dries and pulverizes the solid crude product to form a low-ash biomass carbon precursor material.

2. The method for preparing a low-ash biomass carbon precursor material according to claim 1, characterized in that: The auxiliary agent A is selected from one or more of polyphosphoric acid, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium hydrogen phosphite, ethylenediaminetetraacetic acid, acrylic acid, methacrylic acid, citric acid and tartaric acid, or a combination thereof and an inorganic acid; the fluoride salt compound in the auxiliary agent B is selected from one or more of ammonium fluoride, sodium fluoride and potassium fluoride; the oxidant of the auxiliary agent C is selected from one or more of hydrogen peroxide, sodium peroxide, ammonium persulfate, sodium hypochlorite and sodium perchlorate; the hydrothermal reaction temperature in the step S2 is 160-280°C, and the insulation time is 5-180min.

3. The method for preparing a low-ash biomass carbon precursor material according to claim 1, characterized in that: The auxiliary agent A is one or more of polyphosphoric acid, ethylenediaminetetraacetic acid, acrylic acid, methacrylic acid, citric acid and tartaric acid, or a combination thereof with an inorganic acid; the auxiliary agent C is one or more of hydrogen peroxide, sodium peroxide and ammonium persulfate.

4. The method for preparing a low-ash biomass carbon precursor material according to claim 1, characterized in that: The auxiliary agent A is ethylenediaminetetraacetic acid, the auxiliary agent B is ammonium fluoride or hydrogen fluoride, and the auxiliary agent C is ammonium persulfate.

5. The method for preparing a low-ash biomass carbon precursor material according to claim 4, characterized in that: The hydrothermal reaction temperature is 200-270° C., and the hydrothermal reaction time is 5-120 min.

6. The method for preparing a low-ash biomass carbon precursor material according to claim 1, characterized in that: In the step S2, the amount of the additive A added is 0.1-5wt% of the amount of the biomass raw material in S1, the amount of the additive B added is 0.1-1wt% of the amount of the biomass raw material in S1, and the amount of the additive C added is 0.5-5wt% of the amount of the biomass raw material in S1; the biomass raw material includes one or more combinations of starch, walnut shells, peach pits, bamboo powder, wood powder, bagasse, straw and rice husks; the mass ratio of the biomass raw material to water in the step S1 is 1:1-20.

7. A method for preparing a low-ash hard carbon material, characterized in that: The low-ash biomass carbon precursor material prepared by the method according to any one of claims 1 to 6 is subjected to high-temperature treatment under an inert atmosphere to form a low-ash hard carbon material.

8. The method for preparing a low-ash hard carbon material according to claim 7, characterized in that: The high temperature treatment is to first pre-carbonize at a low temperature of 400-750°C, and then heat up to a high temperature of 1000-1300°C to form a low-ash hard carbon material.

9. The low-ash hard carbon material prepared by the method for preparing a low-ash hard carbon material according to claim 7 or 8.

10. Use of the low-ash hard carbon material according to claim 9 as a negative electrode material for a sodium ion battery.

Citation Information

Patent Citations

  • Biomass charcoal material and preparation method thereof

    CN106829923A

  • Method for preparing carbon cathode for aluminum electrolysis by using waste cathode of aluminum electrolysis cell

    CN110791779A

  • Organic acid modified biomass hard carbon material as well as preparation method and application thereof

    CN117747817A

  • Preparation method and application of coal-based carbon fluoride negative electrode material for sodium ion battery

    CN118083955A

  • Method for removing pyritic, organic, and elemental sulfur from coal

    EP0230500A1