Black silicon dioxide filler as well as preparation method and application thereof
By controlling the water content and heating treatment conditions of the gas atmosphere, a black silica filler with an average particle size of 0.1 to 1 μm was prepared, which solved the dielectric loss and water absorption problems in the prior art, and achieved high dielectric performance and low water absorption characteristics. .
Patent Information
- Application Number
- CN202411246980.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-22
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
AI Technical Summary
The dielectric properties of existing black silica fillers cannot meet the high requirements in the semiconductor field, there is a problem of dielectric loss, and carbon residue leads to high porosity and easy adsorption of moisture in the air.
During the preparation of black silica filler, the water content of the gas atmosphere is controlled, and the heating treatment under an inert gas atmosphere and the calcination under an oxygen-containing gas atmosphere are carried out to prepare black silica with an average particle size of 0.1 to 1 μm. The mass content of carbon in powder gradually increases from the surface to the inside, reducing water absorption and dielectric loss.
The preparation of black silica fillers with excellent dielectric properties is achieved, reducing the dielectric loss of substrate materials, and improving the density and storage resistance of the fillers.
Smart Images

Figure BDA0005031058740000161 
Figure BDA0005031058740000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fillers, and in particular to a black silica filler and a preparation method and application thereof. Background Art
[0002] In the semiconductor field, when passive components, semiconductor components, electroacoustic devices, display devices, optical devices, and radio frequency devices are assembled into devices, circuit board substrate materials such as high-density interconnect boards, high-frequency and high-speed boards, and motherboards are required. These substrate materials are generally composed of fillers and organic polymers such as epoxy resins. The main function of the filler is to reduce the thermal expansion coefficient of the organic polymer, which is mainly angular or spherical silica. In order to facilitate laser printing or reduce light aging, pigments are usually added to the substrate material to dye it gray or black. The commonly used pigment is acetylene black. However, acetylene black is an electronic conductor, and there is a risk of short circuit when it is used as a pigment for substrate materials. Therefore, it is of great significance to prepare black silica and play a dyeing role in the process of filling the substrate material.
[0003] In the prior art, for example, the patent with application publication number CN102924869A discloses a black modified silica, which uses white silica as raw material, carbonizes organic matter at high temperature and adsorbs it in silica. However, it has the following disadvantages: ① The carbon of the black silica is adsorbed on the surface, with more carbon content on the outer surface and less carbon content inside, and the carbon on the surface will aggregate and easily conduct electricity; ② In order to reduce the dielectric properties of black silica, it avoids carbon aggregation by reducing the carbon content, but this will lead to a decrease in the blackness of silica.
[0004] Another example is the patent with application publication number CN113603103A, which provides a semiconductor packaging material and a preparation method thereof. The patent uses polysiloxane particles including T units as the starting raw material particles, and then heat-treats them at 600-800°C in a non-oxidizing gas or vacuum to carbonize the alkyl groups inside the polysiloxane particles and condense the silanol groups on the surface, and then calcines and condenses the remaining silanol groups at 800-1100°C to obtain a semiconductor packaging material, namely black silica powder. The black silica powder provided by the patent has a particle size of 0.8-4.5 μm, but the preparation method has the following problems: the carbon residue in the powder easily causes the silanol groups to form more pores, the porosity is high, and the powder easily absorbs moisture in the air. The powder is used as a filler for substrate materials, which will cause the substrate materials to have a large dielectric loss.
[0005] With the rapid development of microelectronics and communication technology, semiconductor chips are constantly developing towards high integration, miniaturization, high frequency, high power, etc., so higher requirements are also put forward for the dielectric properties of electronic packaging materials. The dielectric properties of existing black silicon dioxide cannot meet the current filler requirements in the semiconductor field. Therefore, a new preparation method of black silicon dioxide is urgently needed to solve the dielectric loss problem of black silicon dioxide. Summary of the invention
[0006] In order to solve the dielectric loss problem of black silica, the present invention provides a black silica filler and a preparation method and application thereof. The present invention prepares a black silica powder with an average particle size of 0.1 to 1 μm by controlling the water in the gas atmosphere during the preparation of the black silica filler.
[0007] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a black silica filler.
[0008] The carbon mass content of the black silicon dioxide filler particles provided by the invention gradually increases from the surface to the inside; the average particle size is 0.1-1 μm, and the carbon mass content is 0.3%-9%.
[0009] Preferably, the carbon content of the black silica filler particles of the present invention is 6% to 9% by mass.
[0010] Preferably, the black silica filler particles of the present invention have a water content of less than 591 ppm / m after being placed at 25°C and 50% RH for 48 hours. 2 .
[0011] Furthermore, from the preparation, the water content is less than 245 ppm / m 2 .
[0012] In the semiconductor field, the filling of substrate materials often requires the use of silica fillers with small particle sizes of 0.5 to 2 μm as the main material for graded filling, while small particles below 0.5 μm can be used for graded filling. In order to play a dyeing role in the process of filling substrate materials, the present invention provides a black silica filler with a single-layer structure, an average particle size of 0.1 to 1 μm, and a carbon mass content of 0.3% to 9%. The filler particles also have other excellent properties, such as: under the environmental conditions of 25°C and 50% RH, after being placed for 48 hours from the preparation, the water content is less than 591ppm / m 2 , has a smaller water absorption capacity, and when it is used as a filler to fill the substrate material, it can make the substrate material have less dielectric loss.
[0013] In the actual application process of silica fillers, they are generally not used directly after preparation, and there is a shelf life, so they will absorb water during storage. The black silica provided by the present invention absorbs less water after storage, which has a great advantage in reducing the dielectric loss caused by water absorption.
[0014] In a second aspect, the present invention provides a method for preparing a black silica filler, specifically: Spherical polysiloxane particles including T units are provided and treated by the following steps: Step S1: performing a heating treatment in an inert gas atmosphere to thermally decompose the organic groups in the particles into carbon; Step S2: calcining the particles in an oxygen-containing gas atmosphere to remove carbon on the particle surface; Wherein, when the temperature of the heating process is controlled to be higher than 650°C, the water content of the inert gas atmosphere is not higher than 3500ppm; the particle size of the black silica filler is 0.1 to 1 μm; Wherein, T unit = R1SiO3-, R1 is a hydrogen atom or an independently selected hydrocarbon group having 1 to 16 carbon atoms.
[0015] The present invention uses polysiloxane containing T units as starting raw material particles, and then heats the particles under an inert gas atmosphere by controlling the temperature to be higher than 650°C and the upper limit of the moisture content in the gas atmosphere to be 3500ppm, so that the organic groups in the particles are thermally decomposed into carbon, and then removes the carbon on the surface of the particles under an oxygen-containing gas atmosphere to obtain a black powder, namely the black silica filler, wherein the average particle size of the black silica filler particles is 0.1 to 1 μm. The advantage of the preparation method provided by the present invention is at least that a black silica filler with a small particle size and excellent dielectric properties can be prepared.
[0016] The biggest reason for the above advantages is that the method of the present invention controls the water content of the gas atmosphere during the heat treatment of the particles, so that the water content of the gas atmosphere is controlled at 3500 ppm or less when the temperature is higher than 650°C.
[0017] The inventors found in the experiment that during the heat treatment of polysiloxane raw material particles, as the silanol condenses, more water will be produced in the particles, including adsorbed water, surface hydroxyl groups, internal hydroxyl groups, etc., so that the gas atmosphere contains a certain concentration of water. At the temperature of the heat treatment, water will react with carbon to take away the carbon in the particles. When the small-particle polysiloxane raw material particles are heat-treated, the existence of this reaction is the main factor limiting the retention of carbon in the particles. When the small-particle polysiloxane raw material particles are heat-treated, if the water concentration of the gas atmosphere during the heat treatment is not controlled, black silicon dioxide cannot be prepared. Therefore, the present invention has conducted further research and found that the minimum temperature for water to react with carbon is about 700°C, and when the temperature is higher than 650°C, the water content of the gas atmosphere of polysiloxane is controlled at 3500ppm or less, which can effectively prevent water from taking away the carbon decomposed from the organic base of the small-particle polysiloxane raw material.
[0018] In large-particle polysiloxane raw material particles, the amount of carbon in the particles is relatively large. After water takes away part of the carbon in the particles, a large amount of carbon can still remain in the particles. Therefore, it is possible to decompose the organic groups without controlling the moisture content of the heat treatment gas atmosphere, and then calcine under oxygen-containing conditions to finally prepare black silica. However, if the moisture concentration of the gas atmosphere during heat treatment is not controlled, only large-particle black silica of more than 5 μm can be prepared, and small-particle black silica cannot be prepared.
[0019] In order to prepare small-particle black silica, the present invention maintains the water content in the gas atmosphere at no more than 3500 ppm when the temperature is higher than 650°C during heat treatment of polysiloxane, thereby reducing the contact between carbon in the silica balls and water and preventing the carbon in the small-particle silica balls from being taken away by water. Then, the carbon on the surface of the silica balls is taken away by calcination under oxygen-containing conditions, and the defects on the surface of the silica balls are repaired by condensation of silanol groups, thereby forming a dense layer on the surface of the silica balls and improving the density of the product, thereby reducing the problem of easy water absorption caused by pores formed by carbon shedding on the surface of the product during the shelf life or use period, and finally preparing black silica filler particles with an average particle size of 0.1 to 1 μm.
[0020] In addition, the black silica filler prepared by the method provided by the present invention has few surface defects, little water absorption, and has the excellent performance of low dielectric loss.
[0021] As a preferred embodiment of the preparation method of the present invention, in step S1, the terminal temperature of the heating treatment is 850-1100°C.
[0022] As a preferred embodiment of the above preparation method of the present invention, the temperature is slowly increased or / and an inert gas is introduced at a high flow rate during the heating process.
[0023] Controlling the moisture content of the gas atmosphere during the heating process is the key to preparing small-particle black silica in the present invention. During the heating process, the moisture content of the gas atmosphere in the heating furnace can be controlled within a relatively low range by slowly increasing the temperature and introducing a high-flow inert gas.
[0024] In order to make the prepared black silica more dense and less water-absorbing, the present invention preferably controls the moisture in the heating furnace within a relatively low range by passing a large flow of nitrogen during the silanol condensation process. The reason is that, in the heating treatment process of step S1 under an inert gas atmosphere, a large flow of nitrogen rapidly takes out the silanol condensation in the polysiloxane raw material to generate moisture, which will affect the arrangement of the R1 group of the T unit, and then affect the overall structural arrangement of the polysiloxane, so that in the back-stage calcination process, the density of the surface dense layer formed by the silanol condensation is higher. The higher density of silica, in the case of the same particle size, has a smaller porosity, that is, a smaller specific surface area, and it is placed in the air for a long time in the later stage, and the water absorption is small. Therefore, the present invention preferably controls the moisture in the heating furnace within a relatively low range by passing a large flow of nitrogen during the silanol condensation process.
[0025] By reducing the heating rate, the condensation rate of silanol in the polysiloxane raw material is reduced, and the rate of generating water is further reduced. The water content in the heat treatment gas atmosphere can also be controlled to be no higher than 3500ppm. However, controlling the water content in this way will easily cause it to burn white in the later calcination process. Alternatively, black silica can be obtained by adjusting the calcination process, but the obtained black silica absorbs a large amount of water after being left for a period of time.
[0026] More preferably, in step S1, the flow rate of the inert gas is 100 to 1000 mL / min.
[0027] The flow rate of the inert gas during heat treatment can be adjusted according to the specific model of the heat treatment device, the amount of heat treatment raw materials, etc., and the water content in the heat treatment gas atmosphere is preferably controlled to be no higher than 3500ppm when the temperature is higher than 650°C.
[0028] More preferably, in step S1, the heating rate of the slow heating is 0.1-1°C / min.
[0029] As a preferred embodiment of the above preparation method of the present invention, in step S2, the volume concentration of oxygen in the oxygen-containing gas is 0.3% to 30%.
[0030] More preferably, in step S2, the volume concentration of oxygen in the oxygen-containing gas is 3% to 21%.
[0031] In step S2, the volume concentration of oxygen in the oxygen-containing gas atmosphere is 3% to 21%, which can achieve a better effect of densification of the particle surface. Along the radial direction of the silica particles, the carbon closer to the surface side is easier to contact with oxygen in the gas atmosphere, and therefore easier to react with it. Therefore, the black silica prepared by the present invention is presumed to have a structure in which the carbon content gradually increases from the surface to the inside, and gradually increases from the surface to the inside with a uniform gradient.
[0032] As a preferred embodiment of the preparation method of the present invention, in step S2, the calcination temperature is 850-1200°C.
[0033] More preferably, in step S2, the calcination treatment time is 0.5 to 72 hours.
[0034] As a preferred embodiment of the above preparation method of the present invention, the polysiloxane further includes Q units, D units and / or M units; wherein, Q unit = SiO4-, D unit = R2R3SiO2-, M unit = R4R5R6SiO-; R2, R3, R4, R5, R6 are respectively hydrogen atoms or independently selectable hydrocarbon groups with 1 to 18 carbon atoms.
[0035] More preferably, the T unit raw material of the polysiloxane is a hydrocarbyltrialkoxysilane or a hydrocarbyltrichlorosilane, the Q unit raw material is at least one selected from the group consisting of tetraalkoxysilane, silicon tetrachloride and silicon dioxide, the D unit raw material is at least one selected from the group consisting of dihydrocarbyldialkoxysilane and dihydrocarbyldichlorosilane, and the M unit raw material is at least one selected from the group consisting of trihydrocarbylalkoxysilane, trihydrocarbylchlorosilane and hexahydrocarbyldisilazane.
[0036] In a third aspect, the present invention provides the use of the above-mentioned black silica filler in the preparation of semiconductor packaging materials and substrate materials.
[0037] In the semiconductor field, the packaging process of semiconductor chips requires the use of semiconductor packaging materials such as plastic packaging materials, patch glue, underfill and chip carrier to package semiconductor chips to protect the chips and provide mechanical support for them. When assembling passive components, semiconductor components, electroacoustic devices, display devices, optical devices and radio frequency devices into equipment, circuit board substrate materials such as high-density interconnect boards, high-frequency and high-speed boards and motherboards are required. For these semiconductor packaging materials and substrate materials, in order to facilitate laser printing on components or laser drilling, or to reduce light aging and improve durability, or to reduce light reflection, or to reduce color changes between batches, they are usually dyed gray or black. In this regard, the industry generally uses acetylene black that does not contain conductive ions as a dye to dye semiconductor packaging materials and substrate materials black, but acetylene black is an electronic conductor, so acetylene black needs to be highly dispersed so that its size is smaller than the metal spacing of semiconductor components to prevent short circuits. However, as the packaging density of semiconductor components increases, the risk of short circuits caused by acetylene black is also increasing. Based on the above preparation method and the above silicon oxide filler, acetylene black can be substituted as a substitute pigment for dyeing semiconductor packaging materials and substrate materials into black, so as to solve the short circuit problem caused by acetylene black. Those skilled in the art can replace acetylene black pigment with the black spherical or amorphous silicon oxide filler provided by the present invention to form semiconductor packaging materials and substrate materials by filling the resin tightly without any creative work. Therefore, these semiconductor packaging materials and substrate materials should also be included in the protection scope of the present invention.
[0038] Preferably, the semiconductor packaging material and substrate material can be used for plastic packaging materials, patch adhesives, underfill materials, chip carriers, circuit boards, or intermediate semi-finished products thereof. The plastic packaging materials are plastic packaging materials in the form of DIP packaging, plastic packaging materials in the form of SMT packaging, MUF, FO-WLP, and FCBGA. Preferably, the circuit board is HDI, a high-frequency high-speed board, or a motherboard.
[0039] Compared with the prior art, the present invention has the following technical effects: (1) The present invention provides a black silica filler having a single-layer structure, an average particle size of 0.1 to 1 μm, and a carbon mass content of 0.3% to 9%, which can be used for grading and tightly filling substrate materials and can also play a dyeing role.
[0040] (2) The black silica filler provided by the present invention has a water content of less than 245 ppm / m after being prepared under the environmental conditions of 25° C. and 50% RH for 48 hours. 2 , has a small water absorption capacity, and when it is used as a filler to fill the substrate material, it can reduce the dielectric loss of the substrate material.
[0041] (3) The present invention also provides a method for preparing black silica filler, which uses polysiloxane containing T units as starting raw material particles, and then controls the temperature to be higher than 650°C and the water content of the gas atmosphere to be no higher than 3500 ppm to heat treat the particles so that the organic groups in the particles are thermally decomposed into carbon, and then calcined in an oxygen-containing gas atmosphere to remove the carbon on the surface of the particles and densify the surface of the particles to obtain small-particle black silica filler with a particle size of 0.1 to 1 μm. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should belong to the scope of protection of the present invention.
[0043] Along the radial direction of the silica particles, the carbon closer to the surface is easier to contact with oxygen in the gas atmosphere and therefore easier to react with it. Therefore, the black silica prepared by the present invention is presumed to have a structure in which the carbon content gradually increases from the surface to the inside and increases from the surface to the inside with a uniform gradient.
[0044] In the semiconductor field, the filling of substrate materials often requires the use of silica fillers with small particle sizes of 0.5 to 2 μm as the main material for graded filling, while small particles below 0.5 μm can be used for graded filling. In order to play a dyeing role in the process of filling substrate materials, the present invention provides a black silica filler with a single-layer structure, an average particle size of 0.1 to 1 μm, and a carbon mass content of 0.3% to 9%. The filler particles also have other excellent properties, such as: under the environmental conditions of 25°C and 50% RH, the water content of the particles as soon as they are prepared is basically 0, and after being placed for 48 hours from the preparation, the water content is less than 591ppm / m 2 It can be seen that the filler particles provided by the present invention have a smaller water absorption capacity. When used as fillers for filling substrate materials, the substrate materials can have less dielectric loss.
[0045] The following examples provide specific implementations of the methods of the present invention, and the detection methods involved include: The moisture content of the particles is the Karl Fischer moisture at 200 degrees Celsius, which is tested using a Karl Fischer titrator.
[0046] The average particle size is measured using a laser particle size distribution analyzer LA-700 from HORIBA. Herein, the average particle size refers to the volume average diameter of the particles.
[0047] The specific surface area was measured using FlowSorbIII2305 produced by SHIMADZU.
[0048] The true specific gravity was measured using MicrotracBEL's BELPycno.
[0049] The uranium and thorium contents were determined using Agilent 7700X ICP-MS. The sample preparation method was to burn at 800°C and then dissolve the sample in hydrofluoric acid.
[0050] The carbon content of silica particles was determined using a CS-8810C carbon-sulfur analyzer from Sichuan Saiens.
[0051] The carbon content on the surface of silica particles was determined by X-ray photoelectron spectroscopy.
[0052] The water content of the gas atmosphere in the muffle furnace is characterized by the water content at the gas outlet of the furnace. In the present invention, the water content of the gas atmosphere during the heat treatment process in the muffle furnace can be replaced by the water content at the gas outlet of the heat treatment furnace being monitored. In the present invention, the heating rate or the gas inlet flow rate or the inlet rate is adjusted so that the maximum water content at the outlet is 3500ppm when the temperature is higher than 650°C, that is, the water concentration in the muffle furnace does not exceed 3500ppm when the temperature is higher than 650°C during the entire heat treatment process.
[0053] The water content at the gas outlet of the heat treatment furnace is tested with a thermometer and hygrometer. The manufacturer of the thermometer and hygrometer is Shenzhen Huahanwei Temperature and Humidity Instrument, model TH11R-EX-H.
[0054] Example 1 Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0055] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1800ppm.
[0056] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0057] The process parameters of heat treatment and calcination are shown in Table 1.
[0058] Example 2 The main difference between this embodiment and embodiment 1 is that the water concentration does not exceed 2500 ppm when the temperature in the muffle furnace is higher than 650° C. during the heat treatment process. The rest is the same as embodiment 1.
[0059] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0060] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 250mL / min, so that the maximum water content at the outlet of the muffle furnace is 2500ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 2500ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 2500ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 2500ppm.
[0061] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to densify the particle surface, thereby obtaining black silica with a carbon mass content that increases uniformly from the surface to the inside.
[0062] The process parameters of heat treatment and calcination are shown in Table 1.
[0063] Example 3 The main difference between this embodiment and embodiment 1 is that the water concentration does not exceed 3500 ppm when the temperature in the muffle furnace is higher than 650° C. during the heat treatment process. The rest is the same as embodiment 1.
[0064] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0065] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 200mL / min, so that the maximum water content at the outlet of the muffle furnace is 3500ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 3500ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is heated to 850℃ at a rate of 5℃ / min, and kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. When the water concentration increases to more than 3500ppm, the nitrogen flow rate is appropriately increased. The present embodiment continuously monitors the water content at the gas outlet of the muffle furnace, and the maximum water content is 3500ppm when the temperature in the muffle furnace is higher than 650℃.
[0066] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to densify the particle surface, thereby obtaining black silica with a carbon mass content that increases uniformly from the surface to the inside.
[0067] The process parameters of heat treatment and calcination are shown in Table 1.
[0068] Example 4 The main difference between this embodiment and embodiment 1 is that the particle size of the polysiloxane raw material in the T unit is 0.73 μm. The other parts are the same as those in embodiment 1.
[0069] Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 60 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 0.73 μm.
[0070] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1800ppm.
[0071] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0072] The process parameters of heat treatment and calcination are shown in Table 1.
[0073] Example 5 The main difference between this embodiment and embodiment 1 is that the particle size of the polysiloxane raw material in the T unit is 0.35 μm. The other parts are the same as those in embodiment 1.
[0074] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 100 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 0.35 μm.
[0075] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1800ppm.
[0076] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0077] The process parameters of heat treatment and calcination are shown in Table 1.
[0078] Example 6 The main difference between this embodiment and embodiment 1 is that the particle size of the polysiloxane raw material in the T unit is 0.18 μm. The other parts are the same as those in embodiment 1.
[0079] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 160 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 0.18 μm.
[0080] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1800ppm.
[0081] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0082] The process parameters of heat treatment and calcination are shown in Table 1.
[0083] Example 7 The main difference between this embodiment and embodiment 1 is that the particle size of the polysiloxane raw material in the T unit is 0.11 μm. The other parts are the same as those in embodiment 1.
[0084] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 160 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 0.11 μm.
[0085] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1800ppm.
[0086] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0087] The process parameters of heat treatment and calcination are shown in Table 1.
[0088] Example 8 The main difference between this embodiment and embodiment 1 is that the means for controlling the moisture content of the gas atmosphere during the heat treatment process is to increase the temperature at a low speed. The rest is the same as embodiment 1.
[0089] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0090] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to 50mL / min, and in a nitrogen atmosphere, heat the furnace temperature at a rate of 1℃ / min to 850℃, keep warm for 10 hours, and heat-treat the particles so that the organic groups in the particles are thermally decomposed into carbon elements. The temperature is raised at a rate of 1℃ / min to ensure that the maximum water content at the outlet is 1800ppm when the furnace temperature is higher than 650℃. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. When the water concentration increases to more than 1800ppm when the furnace temperature is higher than 650℃, the nitrogen flow rate is appropriately increased. The maximum value of the water concentration at the gas outlet of the muffle furnace continuously monitored in this embodiment is 1800ppm, during which the nitrogen flow rate does not exceed 100mL / min, that is, when the temperature in the muffle furnace is higher than 650℃, the water content in the furnace does not exceed 1800ppm.
[0091] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0092] The process parameters of heat treatment and calcination are shown in Table 1.
[0093] Example 9 The main difference between this embodiment and embodiment 1 is that the means for controlling the moisture content of the gas atmosphere during the heat treatment process is to increase the temperature at a low speed, and the calcination treatment time is 0.5 hours. The rest is the same as embodiment 1.
[0094] This example uses polysiloxane containing T units as a starting point to prepare black silica, and the steps are as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0095] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to 50mL / min, and in a nitrogen atmosphere, heat the furnace temperature at a rate of 1℃ / min to 850℃, keep warm for 10 hours, and heat-treat the particles so that the organic groups in the particles are thermally decomposed into carbon elements. The temperature is raised at a rate of 1℃ / min to ensure that the maximum water content at the outlet is 1800ppm when the furnace temperature is higher than 650℃. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. When the water concentration increases to more than 1800ppm when the furnace temperature is higher than 650℃, the nitrogen flow rate is appropriately increased. The maximum value of the water concentration at the gas outlet of the muffle furnace continuously monitored in this embodiment is 1800ppm, during which the nitrogen flow rate does not exceed 100mL / min, that is, when the temperature in the muffle furnace is higher than 650℃, the water content in the furnace does not exceed 1800ppm.
[0096] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 0.5 hours to remove carbon on the particle surface and densify the particle surface to obtain black silica with a carbon mass content that increases uniformly from the surface to the inside.
[0097] The process parameters of heat treatment and calcination are shown in Table 1.
[0098] Example 10 Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0099] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet of the muffle furnace is 1800ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1800ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. When the water concentration increases to more than 1800ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. The present embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace, and the maximum moisture content is 1800ppm when the temperature in the muffle furnace is higher than 650℃.
[0100] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 0.5 hours to remove carbon on the particle surface and densify the particle surface to obtain black silica with a carbon mass content that increases uniformly from the surface to the inside.
[0101] The process parameters of heat treatment and calcination are shown in Table 1.
[0102] Embodiment 11 Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0103] S2, put the spherical polysiloxane powder into the muffle furnace, set the nitrogen flow rate to a larger flow rate, 100mL / min, so that the maximum water content at the outlet of the muffle furnace is 3000ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 3000ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 3000ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 3000ppm.
[0104] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0105] The process parameters of heat treatment and calcination are shown in Table 1.
[0106] Example 12 Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0107] S2, put the spherical polysiloxane powder into the muffle furnace, set the nitrogen flow rate to a larger flow rate, 1000mL / min, so that the maximum water content at the outlet of the muffle furnace is 1400ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 1400ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is raised to 850℃ at a rate of 5℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic groups in the particles are thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 1400ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 1400ppm.
[0108] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to remove carbon on the surface of the particles, densify the surface of the particles, and obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0109] The process parameters of heat treatment and calcination are shown in Table 1.
[0110] Example 13 Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0111] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 100mL / min, so that the maximum water content at the outlet of the muffle furnace is 2000ppm when the temperature in the muffle furnace is higher than 650℃, that is, the moisture content in the muffle furnace does not exceed 2000ppm when the temperature in the muffle furnace is higher than 650℃. Under a nitrogen atmosphere, the temperature in the furnace is heated to 1000℃ at a rate of 10℃ / min, kept warm for 10 hours, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the moisture concentration at the gas outlet of the muffle furnace is continuously monitored. When the moisture concentration increases to more than 2000ppm when the temperature in the furnace is higher than 650℃, the nitrogen flow rate is appropriately increased. This embodiment continuously monitors the moisture content at the gas outlet of the muffle furnace. When the temperature in the muffle furnace is higher than 650℃, the maximum moisture content is 2000ppm.
[0112] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 1200° C. and calcine for 10 hours to remove carbon on the surface of the particles and densify the surface of the particles to obtain black silica with a carbon content that increases uniformly from the surface to the inside.
[0113] The process parameters of heat treatment and calcination are shown in Table 1.
[0114] Comparative Example 1 The main difference from Example 1 is that the nitrogen flow rate during the heat treatment in step S2 is 50 mL / min, so that the water content in the furnace is in the range of 3500 ppm to 4200 ppm.
[0115] The silicon dioxide particles in this comparative example were prepared by the following method: Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0116] S2. Put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to 50 mL / min, raise the temperature in the furnace to 850°C in a nitrogen atmosphere, keep it warm for 10 hours, and heat-treat the particles so that the organic groups in the particles are thermally decomposed into carbon elements. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. In this embodiment, the water concentration at the gas outlet of the muffle furnace is continuously monitored in the range of 2000ppm to 4200ppm. After the temperature in the furnace reaches above 650°C, the water concentration is in the range of 3500ppm to 4200ppm for a total of 5.3 hours.
[0117] S3. Switch the gas in the muffle furnace to air, adjust the temperature to 850° C. and calcine for 3 hours to obtain silicon dioxide particles.
[0118] The process parameters of heat treatment and calcination are shown in Table 1.
[0119] Comparative Example 2 The main difference from Example 1 is that in step S3, the gas is not switched to air. The rest is the same as Example 1.
[0120] The silicon dioxide particles in this comparative example were prepared by the following method: Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0121] S2, put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to a larger flow rate, 300mL / min, so that the maximum water content at the outlet is 1800ppm, that is, during the heat treatment process, when the temperature in the muffle furnace is higher than 650°C, the moisture content in the furnace does not exceed 1800ppm. Under a nitrogen atmosphere, the temperature in the furnace is heated to 850°C at a rate of 5°C / min, and the particles are heat-treated so that the organic base in the particles is thermally decomposed into carbon elements. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. When the water concentration increases to more than 1800ppm when the temperature is higher than 650°C, the nitrogen flow rate is appropriately increased. The present embodiment continuously monitors the water content at the gas outlet of the muffle furnace, and when the temperature in the muffle furnace is higher than 650°C, the maximum water content is 1800ppm.
[0122] S3. Continue calcining for 3 hours to obtain black silica.
[0123] Comparative Example 3 The main difference from Example 1 is that during the heat treatment in step S2, the nitrogen flow rate is 50 mL / min, so that the water content is lower than 4200 ppm when the temperature in the furnace is higher than 650° C.; in step S3, the gas is not switched to air. The rest is the same as Example 1.
[0124] The silicon dioxide particles in this comparative example were prepared by the following method: Starting with a polysiloxane comprising T units, black silica is prepared as follows: S1. Take 1300 parts by weight of deionized water at room temperature and put it into a reactor with a stirrer. Start stirring. Add 200 parts by weight of methyltrimethoxysilane and a small amount of acetic acid to adjust the pH to about 5. After the methyltrimethoxysilane is dissolved, add 30 parts by weight of 5% ammonia water and stir for 10 seconds, then stop stirring. After standing for 1 hour, filter and dry to obtain spherical polysiloxane powder with an average particle size of 1.31 μm.
[0125] S2. Put the spherical polysiloxane powder into a muffle furnace, set the nitrogen flow rate to 50 mL / min, raise the temperature in the furnace to 850°C in a nitrogen atmosphere, keep it warm for 10 hours, and heat-treat the particles so that the organic groups in the particles are thermally decomposed into carbon elements. During the heating process, the water concentration at the gas outlet of the muffle furnace is continuously monitored. In this embodiment, the water concentration at the gas outlet of the muffle furnace is continuously monitored in the range of 2000ppm to 4200ppm. After the temperature in the furnace reaches above 650°C, the water concentration is in the range of 3500ppm to 4200ppm for a total of 5.3 hours.
[0126] S3. Continue calcining for 3 hours to obtain silicon dioxide particles.
[0127] The process parameters of heat treatment and calcination are shown in Table 1.
[0128] Table 1 Process parameters of the embodiments and comparative examples Performance Characterization The silica particles prepared in Examples 1 to 13 and Comparative Examples 1 to 3 were tested for particle size, carbon content, and water content, and the analysis results are shown in Table 2. The 48-hour water content is the water content test conducted after the particles are left open for 48 hours at 25°C and 50% RH from the time of preparation. The 100-day water content is the water content test conducted after the particles are left open for 100 days at 25°C and 50% RH.
[0129] Table 2 Performance characterization results of the examples and comparative examples Data Analysis: ① From the data of Examples 1 to 13, it can be seen that the present invention uses polysiloxane particles including T units as the starting raw material particles, and then heat treats them in an inert gas atmosphere at a temperature higher than 650°C with a water content lower than 3500ppm to thermally decompose the organic groups in the particles into carbon elements, and then calcines them in an oxygen-containing gas atmosphere to densify the particle surface, thereby obtaining a black silica filler with an average particle size of 0.1 to 1 μm. The small-particle black silica filler has the excellent properties of few surface defects and little water absorption after standing.
[0130] ② From the comparative analysis of comparative example 1 and embodiment 1, it can be seen that the main difference between comparative example 1 and embodiment 1 is that when the temperature in the inert gas atmosphere is higher than 650°C, the water content is not higher than 4200ppm, and the carbon content of the obtained silicon dioxide particles is greatly reduced, which shows that the moisture content of the preparation environment needs to be controlled during the heat treatment of small-size carbon-containing particles, otherwise the carbon content of the product will be reduced. Further analysis shows that when the polysiloxane raw material particles are heat treated, with the condensation of silanol groups, more water will be generated in the particles, including adsorbed water, surface hydroxyl groups, internal hydroxyl groups, etc., so that the gas atmosphere contains a certain concentration of water. At the heat treatment temperature, water will react with carbon to take away the carbon in the particles. When the small-size polysiloxane raw material particles are heat treated, the existence of this reaction is the main factor limiting the retention of carbon in the particles. It has been found that the temperature at which water reacts with carbon is about 700°C. Therefore, when the heat treatment decomposes the organic group into carbon, controlling the water concentration at a temperature higher than 650°C can prevent water from taking away the carbon in the particles.
[0131] ③At the same time, from the comparative analysis of Comparative Example 1 and Examples 1 to 3, it can be seen that the main difference between Comparative Example 1 and Examples 1 to 3 is the water content when the temperature in the inert gas atmosphere during heat treatment is higher than 650°C. The black silicon dioxide obtained in Example 1 with the lowest water content during the heat treatment process has the lowest water content after being placed, and the black silicon dioxide obtained in Comparative Example 1 with the highest water content has the highest water content after being placed. This shows that controlling the water content in the environment during the heat treatment process is beneficial to improving the density of the prepared silicon dioxide. Further analysis shows that the reason is that defect sites will be formed after the organic group is converted into carbon. The defect sites have strong water absorption. After the defect sites absorb water, the number of defect points on the surface increases, which in turn leads to a reduction in the surface density of the particles, which is manifested as an increase in the water content of the particles obtained in Comparative Example 1 compared to Examples 1 to 3 after being placed.
[0132] ④ From the comparative analysis of Comparative Example 2 and Example 1, it can be seen that the main difference between Comparative Example 2 and Example 1 is that Comparative Example 2 is calcined in an inert gas atmosphere. The water content of the silica particles obtained in Comparative Example 2 increases greatly after being placed, which shows that if the particles are not calcined in an oxygen-containing atmosphere, the surface of the particles cannot be densified, which will lead to an increase in the water absorption of the product after placement. Further analysis shows that the reason is that by calcining under oxygen-containing conditions, the carbon on the surface of the silica sphere can be taken away, and the defects on the surface of the silica sphere can be repaired by condensation of silanol groups, forming a dense layer on the surface of the silica sphere, improving the density of the product, and thus avoiding the problem of easy water absorption caused by the shedding of carbon on the surface of the product during the shelf life or use period to form pores.
[0133] ⑤ From the comparative analysis of Comparative Example 1, Comparative Example 3 and Example 1, it can be seen that the main difference between Comparative Example 3 and Example 1 is that the water content in the inert gas atmosphere during heat treatment reaches 4200ppm, the water content is relatively large, and calcination is carried out in an inert gas atmosphere; the main difference between Comparative Example 3 and Comparative Example 1 is that Comparative Example 3 is calcined in an inert gas atmosphere; the difference between Comparative Example 1 and Example 1 is mainly that the water content in the inert gas atmosphere during heat treatment of Comparative Example 1 reaches 4200ppm, and the water content is relatively large. From the performance characterization results of the three products, it can be seen that although the carbon content of Comparative Example 1 is small, its water content is not significantly increased compared with Example 1, indicating that the moisture control of the gas atmosphere during heat treatment mainly affects the carbon content of the product; the carbon content of Comparative Example 3 is significantly smaller than that of Example 1, and the water content after placement is also significantly increased, that is, the density of the product decreases, which indicates that the density of the product surface is affected by the calcination atmosphere.
[0134] ⑥ From the comparative analysis of Example 8 and Example 9 with Example 1, it can be seen that the main difference between Example 8 and Example 1 is that the means of controlling the moisture concentration of the heat treatment gas atmosphere is slow heating. The product characterization results of Example 8 show that the carbon content is reduced to a certain extent and the water absorption is greatly increased after being placed, which shows the advantage of achieving low moisture concentration of the gas atmosphere by rapid purging of large flow nitrogen. Example 9 can increase the carbon content of the product to a certain extent compared with Example 8 by shortening the calcination time in the oxygen atmosphere, but the water absorption is still greatly increased after being placed.
[0135] The reason for the advantage of achieving low moisture concentration in the gas atmosphere by rapid purging with high-flow nitrogen is that during the heating process under an inert gas atmosphere, high-flow nitrogen quickly removes moisture generated by condensation of silanol groups in the polysiloxane raw material, which affects the arrangement of the R1 group of the T unit, and further affects the overall structural arrangement of the polysiloxane, making the surface dense layer formed by condensation of silanol groups higher in density in the later calcination process. Silica with higher density has a smaller porosity, that is, a smaller specific surface area, at the same particle size, and absorbs less water when placed in the air for a long time in the later stage.
[0136] The uranium and thorium contents of all samples of Examples 1 to 13 are less than 1 ppb. The samples of Examples 1 to 13 can be surface treated. Specifically, vinyl silane coupling agent, epoxy silane coupling, disilazane, etc. can be used for treatment as needed. More than one treatment can be used as needed.
[0137] The "main powder" mentioned in the present invention refers to the powder of large particle segments of the total filler filled in the resin.
[0138] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0139] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A black silica filler, characterized in that: The mass content of carbon in the black silica filler particles gradually increases from the surface to the inside; The average particle size of the black silica filler particles is 0.1-1 μm, and the mass content of carbon is 0.3%-9%.
2. The black silica filler according to claim 1, characterized in that: From the preparation, under the environmental conditions of 25°C and 50% RH, the water content of the black silica filler particles is less than 591 ppm / m 2 .
3. The black silica filler according to claim 1, characterized in that: From the preparation, under the environmental conditions of 25°C and 50% RH, the water content of the black silica filler particles is less than 245 ppm / m 2 .
4. A method for preparing a black silica filler, characterized in that: Spherical polysiloxane particles including T units are provided and treated by the following steps: Step S1: performing a heating treatment in an inert gas atmosphere to thermally decompose the organic groups in the particles into carbon; Step S2: calcining the particles in an oxygen-containing gas atmosphere to remove carbon on the particle surface; Wherein, when the temperature of the heating process is controlled to be higher than 650°C, the water content of the inert gas atmosphere is not higher than 3500ppm; the particle size of the black silica filler is 0.1 to 1 μm; Wherein, T unit = R1SiO3-, R1 is a hydrogen atom or an independently selected hydrocarbon group having 1 to 16 carbon atoms.
5. The method for preparing a black silica filler according to claim 4, characterized in that: In step S1, the terminal temperature of the heating treatment is 850-1100°C.
6. The method for preparing a black silica filler according to claim 5, characterized in that: During the heating process, the temperature is increased slowly or / and an inert gas is introduced at a high flow rate.
7. The method for preparing a black silica filler according to claim 6, characterized in that: The slow heating rate is 0.1-1°C / min.
8. The method for preparing a black silica filler according to claim 6, characterized in that: The flow rate of the inert gas is 100-1000 mL / min.
9. The method for preparing a black silica filler according to claim 4, characterized in that: In step S2, the volume concentration of oxygen in the oxygen-containing gas is 0.3% to 30%.
10. The method for preparing a black silica filler according to claim 9, characterized in that: In step S2, the volume concentration of oxygen in the oxygen-containing gas is 3% to 21%.
11. The method for preparing a black silica filler according to claim 4, characterized in that: In step S2, the calcination temperature is 850-1200°C.
12. The method for preparing a black silica filler according to claim 4, characterized in that: The polysiloxane further comprises Q units, D units and / or M units; wherein Q units = SiO4-, D units = R2R3SiO2-, and M units = R4R5R6SiO-; R2, R3, R4, R5 and R6 are each a hydrogen atom or an independently selected hydrocarbon group having 1 to 18 carbon atoms.
13. The method for preparing a black silica filler according to claim 12, characterized in that: The T unit raw material of the polysiloxane is a hydrocarbyltrialkoxysilane or a hydrocarbyltrichlorosilane, the Q unit raw material is selected from at least one of the group consisting of tetraalkoxysilane, silicon tetrachloride and silicon dioxide, the D unit raw material is selected from at least one of the group consisting of dihydrocarbyldialkoxysilane and dihydrocarbyldichlorosilane, and the M unit raw material is selected from at least one of the group consisting of trihydrocarbylalkoxysilane, trihydrocarbylchlorosilane and hexahydrocarbyldisilazane.
14. Use of the black silica filler according to any one of claims 1 to 3, or the black silica filler prepared by the preparation method according to any one of claims 4 to 13 in the preparation of semiconductor packaging materials or substrate materials.
Citation Information
Patent Citations
Black powder, and method for producing same
CN111032570A
Preparation method of spherical silicon dioxide powder filler, powder filler obtained by preparation method and application thereof
CN112236393A
Preparation method of hollow silicon dioxide powder filler, powder filler obtained by preparation method and application of powder filler
CN112624126A
Preparation method of silicon dioxide powder filler, powder filler obtained through preparation method and application of powder filler
CN112812361A
Preparation method of semiconductor packaging material and substrate material, semiconductor packaging material and substrate material obtained thereby, and application of semiconductor packaging material and substrate material