Treatment method of electrolytic aluminum solid waste
Through the sorting, flotation and medium-temperature activation treatment of electrolytic aluminum solid waste, the problem of handling harmful substances in solid waste is solved, the recycling of aluminum fluoride and activated carbon is realized, and environmental pollution and costs are reduced.
Patent Information
- Application Number
- CN202411098190.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
The harmful substances in the solid waste generated during the electrolytic aluminum production process are difficult to effectively deal with, traditional recycling efficiency is low, there is a risk of fluorine pollution, and the treatment cost is high.
The electrolytic aluminum solid waste is treated by steps such as sorting, flotation and medium temperature activation. Through coarse grinding, sorting, mixing, flotation, activation and other processes, aluminum fluoride and activated carbon are recovered to reduce the pollution of harmful substances.
It realizes the effective recycling and utilization of valuable elements in solid waste, reduces environmental pollution, improves resource utilization efficiency, reduces raw material and energy consumption, and reduces corporate costs.
Smart Images

Figure CN118929720A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrolytic aluminum waste treatment, and in particular to a method for treating electrolytic aluminum solid waste. Background Art
[0002] Aluminum electrolyte waste slag, carbon slag and overhaul slag are the three main types of solid wastes generated in the electrolytic aluminum production process.
[0003] In the process of electrolytic aluminum production, as the alumina raw materials are consumed, alkali metal impurities such as Li, Na, and K continue to accumulate in the aluminum electrolyte, resulting in a decrease in the primary crystallization temperature of the aluminum electrolyte melt and a decrease in the ability to dissolve the alumina raw materials, which leads to problems such as difficulty in electrolytic cell operation, reduced current efficiency, and increased energy consumption. In order to maintain the normal operation of electrolytic aluminum production, it is necessary to continuously remove alkali metal-rich aluminum electrolyte waste slag from the aluminum electrolytic cell. Aluminum electrolyte waste slag contains a large amount of fluoride, which poses a risk of fluorine pollution diffusion and is a large amount of hazardous waste that needs to be treated urgently.
[0004] There are two main types of carbon slag: one is the waste slag formed by the uneven combustion and selective oxidation of the anode carbon rod in the electrolytic cell during the production of electrolytic aluminum, which causes the carbon particles to fall off; the other is the carbon particles produced by the cathode carbon block being eroded and washed by aluminum liquid and electrolyte during the aluminum electrolysis process. Due to the immersion and penetration of the electrolyte, the carbon slag generally contains 20% to 30% carbon and 60% to 70% electrolyte.
[0005] Overhaul slag is the waste or by-product generated during the large-scale maintenance, renovation or reconstruction of equipment or engineering facilities in the electrolytic aluminum production process. It mainly includes carbonaceous solid waste composed of spent cathode carbon blocks, edge carbon bricks and inter-paste materials, and non-carbonaceous solid waste formed by refractory materials of the tank lining. At present, the amount of overhaul slag generated for every ton of aluminum produced is approximately 22kg to 25kg.
[0006] At present, aluminum enterprises use methods such as pyrolysis to treat the above electrolyte solid waste, but the traditional methods have very limited efficiency in recovering effective elements in solid waste. Therefore, traditional technologies still need to be improved. Summary of the invention
[0007] Based on this, one or more embodiments of the present application provide a method for treating electrolytic aluminum solid waste that can effectively remove harmful substances in solid waste and achieve the recycling of valuable elements.
[0008] According to a first aspect of an embodiment of the present application, a method for treating solid waste from electrolytic aluminum is provided, comprising the following steps:
[0009] Providing aluminum electrolysis solid waste, wherein the aluminum electrolysis solid waste includes aluminum waste electrolyte, carbon slag and overhaul slag;
[0010] The overhaul slag is subjected to coarse grinding and sorting treatment in sequence to obtain non-carbonaceous solid waste and carbonaceous solid waste;
[0011] Mixing the carbonaceous solid waste, the waste aluminum electrolyte and the carbon slag to obtain a first mixture;
[0012] performing flotation treatment on the first mixture to obtain spent electrolyte and carbon powder; and
[0013] The waste electrolyte and the composite activator are mixed, and medium-temperature activation treatment and filtration treatment are performed in sequence to obtain aluminum fluoride and a filtrate.
[0014] In one embodiment, the treatment method further comprises the following steps: sequentially performing carbonization treatment and activation treatment on the carbon powder to obtain activated carbon;
[0015] Optionally, the temperature of the carbonization treatment is 300° C. to 600° C., and the time of the carbonization treatment is 0.5 h to 1.5 h;
[0016] Optionally, the activation treatment temperature is 600° C. to 900° C.;
[0017] Optionally, the activation gas for the activation treatment is selected from one or more of water vapor, carbon dioxide and air.
[0018] In one embodiment, the treatment method further comprises the following steps: grinding the non-carbonaceous solid waste to a particle size of 0.5 mm to 1.5 mm, mixing the non-carbonaceous solid waste with the activated carbon, and sequentially performing hydration treatment, filtering treatment and drying treatment to obtain a refractory material raw material;
[0019] Optionally, the hydration treatment time is 0.5h to 1.5h;
[0020] Optionally, the mixing mass ratio of the non-carbonaceous solid waste to the activated carbon is 1:(0.3-0.5);
[0021] Optionally, the water temperature in the hydration treatment is 30°C to 50°C.
[0022] In one embodiment, the treatment method further comprises the following steps: drying the filtrate to obtain sodium salt.
[0023] In one of the embodiments, the mass ratio of the carbonaceous solid waste, the waste aluminum electrolyte and the carbon slag is 1:(2-3):(2-3).
[0024] In one of the embodiments, the mass ratio of the waste electrolyte to the composite activator is 1:(0.3-0.7).
[0025] In one embodiment, before flotation of the first mixture, the following step is further included: fine grinding the first mixture to a particle size of 0.04 mm to 0.1 mm.
[0026] In one embodiment, the composite activator is selected from two or more of aluminum sulfate, aluminum nitrate, aluminum carbonate, aluminum chloride, sodium aluminate and sodium aluminate.
[0027] In one embodiment, the temperature of the medium-temperature activation treatment is 450° C. to 650° C.; the time of the medium-temperature activation treatment is 0.5 h to 1.5 h.
[0028] In one embodiment, the processing method satisfies at least one of the following conditions:
[0029] (1) The pulp concentration in the flotation process is 15wt% to 35wt%; the rotation speed of the flotation process is 1000rpm to 3000rpm; the aeration volume of the flotation process is 150L / min to 350L / min;
[0030] (2) the inhibitor of the flotation treatment is selected from one or more of lime, sodium carbonate and water glass;
[0031] (3) the collector of the flotation treatment is selected from one or more of light diesel, kerosene and gasoline; and
[0032] (4) The frother of the flotation treatment is selected from one or more of No. 2 oil, eucalyptus oil and camphor oil.
[0033] Compared with the traditional technology, this application has the following beneficial effects:
[0034] The method for treating electrolytic aluminum solid waste provided in the present application can effectively recover aluminum fluoride from solid waste and realize the recycling of resources by sorting, flotation, medium-temperature activation and other treatments of solid waste based on the synergistic effect between the above steps; at the same time, it can reduce the harm of harmful substances in solid waste to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0036] Figure 1 This is a schematic diagram of the treatment process of solid waste from electrolytic aluminum in one embodiment of the present application. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present application, etc. can be purchased from the market or can be prepared by existing methods.
[0039] Some embodiments of the present application provide a method for treating solid waste from electrolytic aluminum, including steps S1 to S3 and steps S5 to S7.
[0040] Step S1: providing aluminum electrolysis solid waste, wherein the aluminum electrolysis solid waste includes aluminum waste electrolyte, carbon slag and overhaul slag;
[0041] Step S2: performing coarse grinding and sorting on the overhaul slag in sequence to obtain non-carbonaceous solid waste and carbonaceous solid waste;
[0042] Step S3: mixing carbonaceous solid waste, waste aluminum electrolyte and carbon slag to obtain a first mixture;
[0043] Step S5: performing flotation treatment on the first mixture to obtain spent electrolyte and carbon powder; and
[0044] Step S6: mixing the waste electrolyte and the composite activator, and performing a medium-temperature activation treatment to obtain a second mixture;
[0045] Step S7: filtering the second mixture to obtain aluminum fluoride and a filtrate.
[0046] In some embodiments, in step S2, a jaw crusher or a vertical impact crusher is used to coarsely grind the overhaul slag.
[0047] In some embodiments, in step S2, the particle size of the overhaul slag after the rough grinding treatment is 3 mm to 5 mm, for example, 3 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.9 mm, 4.0 mm, 4.1 mm, 4.2 mm, 4.3 mm, 4.4 mm, 4.5 mm, 4.6 mm, 4.7 mm, 4.8 mm, 4.9 mm or 5.0 mm.
[0048] In some embodiments, in step S2, the overhaul slag after the rough grinding process is sorted using a color sorting device. It can be understood that the sorting process is based on the color difference of different materials to obtain non-carbonaceous solid waste and carbonaceous solid waste. Non-carbonaceous solid waste and carbonaceous solid waste often have obvious differences in color, and the color sorting device can identify and separate wastes of different colors.
[0049] In some embodiments, in step S3, the mass ratio of carbonaceous solid waste, waste aluminum electrolyte and carbon slag is 1:(2-3):(2-3). For example, it can be 1:2:2, 1:2:3, 1:3:3, 1:3:2 or 1:2.5:2.5.
[0050] In some embodiments, in step S3, the mixing time is 0.4 h to 0.6 h; optionally 0.5 h.
[0051] In some embodiments, after step S3 and before step S5, step S4 is further included: finely grinding the first mixture to a particle size of 0.04 mm to 0.1 mm. It is understood that the particle size of the first mixture after fine grinding can be 0.04 mm, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm or 0.1 mm.
[0052] It is understandable that if the particle size of the carbonaceous solid waste, the waste aluminum electrolyte and the carbon slag after mixing is 0.04 mm to 0.1 mm, there is no need to perform fine grinding treatment on the first mixture separately.
[0053] In some embodiments, in step S5, the flotation process includes one roughing and three scavenging processes, that is, a "one roughing and three scavenging" process.
[0054] In a specific example, the flotation treatment includes the following steps: adding the first mixture into water, placing it in a flotation tank, adjusting the speed of the flotation machine to be stable, and then stirring it in air to allow the slurry to be fully mixed, and then adding an inhibitor, a collector and a frother in sequence, controlling the scraper speed, and adjusting the inflation volume before flotation to obtain waste electrolyte and carbon powder.
[0055] In some embodiments, in step S5, the pulp concentration in the flotation process is 15% to 35%; for example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34% or 35%.
[0056] In some embodiments, in step S5, the rotation speed of the flotation treatment is 1000rpm to 3000rpm; for example, it can be 1000rpm, 1100rpm, 1200rpm, 1300rpm, 1400rpm, 1500rpm, 1600rpm, 1700rpm, 1800rpm, 1900rpm, 2000rpm, 2100rpm, 2200rpm, 2300rpm, 2400rpm, 2500rpm, 2600rpm, 2700rpm, 2800rpm, 2900rpm or 3000rpm.
[0057] In some embodiments, in step S5, the aeration rate of the flotation treatment is 150L / min to 350L / min; for example, it can be 150L / min, 160L / min, 170L / min, 180L / min, 190L / min, 200L / min, 210L / min, 220L / min, 230L / min, 240L / min, 250L / min, 260L / min, 270L / min, 280L / min, 290L / min, 300L / min, 310L / min, 320L / min, 330L / min, 340L / min or 350L / min.
[0058] In some embodiments, in step S5, the inhibitor of the flotation treatment is selected from one or more of lime, sodium carbonate and water glass.
[0059] In some embodiments, in step S5, the collector for flotation treatment is selected from one or more of light diesel oil, kerosene and gasoline.
[0060] In some specific examples, the collector of the flotation process is selected from kerosene and gasoline. Optionally, the mass ratio of gasoline to kerosene is 1:2.
[0061] In some embodiments, in step S5, the frother of the flotation treatment is selected from one or more of No. 2 oil, eucalyptus oil and camphor oil.
[0062] In some embodiments, in step S6, the mass ratio of the waste electrolyte to the composite activator is 1:(0.3-0.7), for example, 1:0.3, 1:0.4, 1:0.5, 1:0.6 or 1:0.7.
[0063] In some embodiments, in step S6, the composite activator is selected from two or more of aluminum sulfate, aluminum nitrate, aluminum carbonate, aluminum chloride, sodium aluminate and potassium aluminate. It can be selected from one or more of the following combinations: aluminum sulfate + sodium aluminate, aluminum nitrate + sodium aluminate, aluminum carbonate + potassium aluminate, aluminum chloride + potassium aluminate, aluminum sulfate + aluminum nitrate + sodium aluminate, aluminum nitrate + sodium aluminate + potassium chlorate.
[0064] In some specific examples, the composite activator is selected from aluminum carbonate and potassium aluminate; optionally, the mass ratio of aluminum carbonate to potassium aluminate is 1:0.5.
[0065] In some embodiments, in step S6, the temperature of the medium temperature activation treatment is 450°C to 650°C. For example, it can be 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C or 650°C.
[0066] In some embodiments, in step S6, the time of the medium-temperature activation treatment is 0.5 h to 1.5 h; for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h or 1.5 h.
[0067] It is understandable that the solid waste of electrolytic aluminum can be converted into aluminum fluoride through the above steps of the present application, thereby realizing the recycling of resources. At the same time, the aluminum fluoride obtained by the above method of the present application has the advantages of low loss on ignition.
[0068] In some embodiments, the above-mentioned treatment method further includes step S8: drying the filtrate to obtain sodium salt.
[0069] In some embodiments, in step S8, the temperature of the drying process is 105°C to 115°C, and can be 110°C.
[0070] It can be understood that the main chemical component of the filtrate obtained by filtration in step S7 includes sodium, and sodium salt can be obtained by drying it, thereby realizing the recycling of resources.
[0071] In some embodiments, the above-mentioned treatment method further includes step S9: sequentially performing carbonization treatment and activation treatment on the carbon powder to obtain activated carbon.
[0072] In some embodiments, in step S9, the temperature of the carbonization treatment is 300°C to 600°C; for example, it can be 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C.
[0073] In some embodiments, in step S9, the carbonization treatment time is 0.5h to 1.5h; for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h.
[0074] In some embodiments, in step S9, the temperature of the activation treatment is 600°C to 900°C; for example, it can be 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C, 800°C, 820°C, 840°C, 860°C, 880°C or 900°C.
[0075] In some embodiments, in step S9, the activation gas for the activation treatment is selected from one or more of water vapor, carbon dioxide and air.
[0076] It can be understood that the carbon powder obtained by flotation can be converted into activated carbon by carbonizing and activating it, thereby realizing resource recycling.
[0077] In some of the embodiments, the above-mentioned treatment method further includes step S11: mixing the non-carbonaceous solid waste with the activated carbon obtained in step S9, and sequentially performing hydration treatment, filtering treatment and drying treatment to obtain a refractory material raw material.
[0078] Furthermore, in step S11, the non-carbonaceous solid waste obtained by sorting in step S2 is mixed with the activated carbon obtained in step S9, and then hydrated, filtered and dried to prepare a refractory raw material. Among them, the activated carbon can remove harmful elements such as cyanide in the non-carbonaceous solid waste. The refractory raw material includes Al 2 O 3 、SiO 2 、Si 3 N 4 and SiC.
[0079] In some embodiments, in step S11, the mixing mass ratio of the non-carbonaceous solid waste to the activated carbon is 1:(0.3-0.5), for example, 1:0.3, 1:0.35, 1:0.4, 1:0.45 or 1:0.5.
[0080] In some embodiments, in step S11, the water temperature during the hydration treatment is 30°C to 50°C. For example, it can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C.
[0081] In some embodiments, in step S11, the hydration treatment time is 0.5 h to 5 h; for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 2 h, 3 h, 4 h or 5 h.
[0082] In some embodiments, before mixing the non-carbonaceous solid waste with the activated carbon, the step S10 is further included: grinding the non-carbonaceous solid waste to a particle size of 0.5 mm to 1.5 mm, for example, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm or 1.5 mm.
[0083] It is understandable that if the particle size of the non-carbonaceous solid waste obtained after sorting is 0.5 mm to 1.5 mm, there is no need to perform fine grinding treatment on the non-carbonaceous solid waste separately.
[0084] The present application targets three types of solid waste generated in the electrolytic aluminum reaction, and based on the steps of sorting, flotation and medium-temperature activation, uses color sorting to separate non-carbonaceous solid waste and carbonaceous solid waste; the carbonaceous solid waste is mixed with waste aluminum electrolyte and carbon slag and separated by flotation to obtain carbon powder and waste electrolyte, which are then reacted with a composite activator to produce aluminum fluoride; the carbon powder is carbonized and activated to become activated carbon, which can be used to remove harmful elements such as cyanide from the non-carbonaceous solid waste.
[0085] The above-mentioned method of the present application is used to treat the solid waste from the electrolytic aluminum reaction. The various steps cooperate and work synergistically with each other, thereby reducing the pollution of the waste to the environment, which is beneficial to protecting the environment and the ecosystem; at the same time, it realizes the effective recovery of useful substances in the electrolyte, carbon slag and overhaul slag, reduces the consumption of raw materials and energy, and improves the efficiency of resource utilization; after resource processing, recycled products or by-products can be obtained, which increases economic benefits.
[0086] Compared with the traditional method of separately treating different types of solid waste, the method of the present application can achieve simultaneous treatment of three types of solid waste, thereby reducing the investment cost and operation cost of the enterprise.
[0087] The above method of the present application has the advantages of simple process, green environmental protection, safety and health.
[0088] The present application will be further described below in conjunction with specific examples and comparative examples, but they should not be construed as limiting the scope of protection of the present application. The raw materials involved in the following specific examples, unless otherwise specified, can all be sourced from commercial sources, the instruments used, unless otherwise specified, can all be sourced from commercial sources, and the processes involved, unless otherwise specified, are all conventionally selected by those skilled in the art.
[0089] Example 1
[0090] according to Figure 1 The process shown is used to treat the overhaul slag, carbon slag and waste aluminum electrolyte produced by the aluminum electrolysis reaction. The specific steps are as follows:
[0091] (1) The overhaul slag is placed in a crusher for coarse crushing to obtain overhaul slag with a particle size of 5 mm.
[0092] (2) The overhaul slag after crushing and screening is automatically sorted by a color sorter according to the color difference of different materials to obtain carbonaceous solid waste (selected material A) and non-carbonaceous solid waste (selected material B).
[0093] (3) mixing the selected material A obtained by sorting in step (2) and the waste electrolyte and carbon slag produced by aluminum electrolysis at a mass ratio of 1:2:2 for 0.5 h to obtain a first mixture; and finely grinding the first mixture to a particle size of 0.1 mm;
[0094] The first mixture after fine grinding is floated: the mixture is added into water, placed in a flotation tank, the speed of the flotation machine is adjusted to be stable, and then air stirring is performed to make the slurry fully mixed, and then the inhibitor, collector and foaming agent are added in sequence, the scraper speed is controlled, and the aeration volume is adjusted before flotation to obtain waste electrolyte (floating material C) and carbon powder (floating material D). Among them, the ore pulp concentration is 15wt%, the speed of the flotation machine is 1000rpm, and the aeration volume of the flotation machine is selected to be 150L / min. Among them, the inhibitor is selected from water glass; the collector is selected from gasoline and kerosene (the mass ratio of gasoline to kerosene is 1:2); the foaming agent is selected from No. 2 oil.
[0095] (4) drying the flotation material C obtained in step (3) and mixing it with a composite activator at a mass ratio of 1:0.3, placing it in a crucible after mixing for 0.5 h, and performing medium-temperature activation treatment in a heating furnace. After the reaction is completed, filtering is performed, and the filter residue is dried to obtain aluminum fluoride, and the filtrate is dried at 110° C. to obtain sodium salt. The temperature of the medium-temperature activation treatment is 450° C., and the reaction time is 0.5 h; the composite activator is selected from aluminum sulfate and sodium aluminate (the mass ratio of aluminum sulfate to sodium aluminate is 1:0.5).
[0096] (5) The flotation material D obtained in step (3) is first dried in an air-tight environment at a temperature of 120° C. for 0.5 h, and then the temperature is further raised to 300° C. for carbonization for 0.5 h; after the carbonization is completed, an activation gas is introduced for activation treatment, the temperature is controlled at 600° C., and the activation gas is air; after the activation is completed, the activated material is cooled with circulating water to obtain activated carbon.
[0097] (6) Finely grind the selected material B obtained in step (2) to a particle size of about 1.5 mm, mix the finely ground powder with activated carbon in a mass ratio of 1:0.3, add the powder into water and stir for hydration treatment, the water temperature is 30°C, and the stirring time is 0.5 h; after hydration treatment, filter and dry to obtain a refractory raw material.
[0098] Example 2
[0099] (1) The overhaul slag is placed in a crusher for coarse crushing to obtain overhaul slag with a particle size of 2 mm.
[0100] (2) The overhaul slag after crushing and screening is automatically sorted by a color sorter according to the color difference of different materials to obtain carbonaceous solid waste (selected material A) and non-carbonaceous solid waste (selected material B).
[0101] (3) mixing the selected material A obtained by sorting in step (2) and the waste electrolyte and carbon slag produced by aluminum electrolysis at a mass ratio of 1:4:4 for 0.5 h to obtain a first mixture; and finely grinding the first mixture to a particle size of 0.2 mm;
[0102] The first mixture after fine grinding is floated: the mixture is added into water, placed in a flotation tank, the speed of the flotation machine is adjusted to be stable, and then stirred in air to make the slurry fully mixed, and then the inhibitor, collector and frother are added in sequence, the scraper speed is controlled, and the aeration volume is adjusted before flotation to obtain waste electrolyte (flotation material C) and carbon powder (flotation material D). Among them, the ore pulp concentration is 10%, the speed of the flotation machine is 500rpm, and the aeration volume of the flotation machine is selected to be 100L / min. Among them, the inhibitor is selected from water glass; the collector is selected from gasoline and kerosene (the mass ratio of gasoline to kerosene is 1:2); the frother is selected from No. 2 oil.
[0103] (4) drying the flotation material C obtained in step (3) and mixing it with a composite activator at a mass ratio of 1:0.8, placing it in a crucible after mixing for 0.5 hours, and performing medium-temperature activation treatment in a heating furnace. After the reaction is completed, filtering is performed, and the filter residue is dried to obtain aluminum fluoride, and the filtrate is dried at 110° C. to obtain sodium salt. The temperature of the medium-temperature activation treatment is 750° C., and the reaction time is 3 hours; the composite activator is selected from aluminum sulfate and sodium aluminate (the mass ratio of aluminum sulfate to sodium aluminate is 1:0.5).
[0104] (5) The flotation material D obtained in step (3) is first dried in an air-tight environment at a temperature range of 100° C. to 120° C. for 0.5 h, and then the temperature is raised to 250° C. for carbonization for 0.5 h; after the carbonization is completed, an activation gas is introduced for activation treatment, the temperature is controlled at 450° C., and the activation gas is air; after the activation is completed, the activated material is cooled with circulating water to obtain activated carbon.
[0105] (6) Finely grind the selected material B obtained in step (2) to a particle size of about 2 mm, mix the finely ground powder with activated carbon in a mass ratio of 1:0.1, add the mixture into water and stir for hydration treatment, the water temperature is 25°C, and the stirring time is 0.5 h; after hydration treatment, filter and dry to obtain a refractory raw material.
[0106] Example 3
[0107] (1) The overhaul slag is placed in a crusher for coarse crushing to obtain overhaul slag with a particle size of 6 mm.
[0108] (2) The overhaul slag after crushing and screening is automatically sorted by a color sorter according to the color difference of different materials to obtain carbonaceous solid waste (selected material A) and non-carbonaceous solid waste (selected material B).
[0109] (3) mixing the selected material A obtained by sorting in step (2) and the waste electrolyte and carbon slag produced by aluminum electrolysis at a mass ratio of 1:1:1 for 0.5 h to obtain a first mixture; and finely grinding the first mixture to a particle size of 0.2 mm;
[0110] The first mixture after fine grinding is floated: the mixture is added into water, placed in a flotation tank, the speed of the flotation machine is adjusted to be stable, and then stirred in air to make the slurry fully mixed, and then the inhibitor, collector and frother are added in sequence, the scraper speed is controlled, and the aeration volume is adjusted before flotation to obtain waste electrolyte (flotation material C) and carbon powder (flotation material D). Among them, the ore pulp concentration is 40%, the speed of the flotation machine is 4000rpm, and the aeration volume of the flotation machine is selected to be 450L / min. Among them, the inhibitor is selected from water glass; the collector is selected from gasoline and kerosene (the mass ratio of gasoline to kerosene is 1:2); the frother is selected from No. 2 oil.
[0111] (4) drying the flotation material C obtained in step (3) and mixing it with a composite activator at a mass ratio of 1:0.2, placing it in a crucible after mixing for 0.5 hours, and performing medium-temperature activation treatment in a heating furnace. After the reaction is completed, filtering is performed, and the filter residue is dried to obtain aluminum fluoride, and the filtrate is dried at 110° C. to obtain sodium salt. The temperature of the medium-temperature activation treatment is 350° C., and the reaction time is 0.5 hours; the composite activator is selected from aluminum sulfate and sodium aluminate (the mass ratio of aluminum sulfate to sodium aluminate is 1:0.5).
[0112] (5) The flotation material D obtained in step (3) is first dried in an air-tight environment at a temperature of 120° C. for 0.5 h, and then the temperature is further raised to 200° C. for carbonization for 0.5 h; after the carbonization is completed, an activation gas is introduced for activation treatment, the temperature is controlled at 500° C., and the activation gas is air; after the activation is completed, the activated material is cooled with circulating water to obtain activated carbon.
[0113] (6) Finely grind the selected material B obtained in step (2) to a particle size of about 2 mm, mix the finely ground powder with activated carbon in a mass ratio of 1:0.2, add the powder into water and stir for hydration treatment, the water temperature is 20°C, and the stirring time is 0.5 h; after hydration treatment, filter and dry to obtain a refractory raw material.
[0114] Example 4
[0115] (1) The overhaul slag is placed in a crusher for coarse crushing to obtain overhaul slag with a particle size of 5 mm.
[0116] (2) The overhaul slag after crushing and screening is automatically sorted by a color sorter according to the color difference of different materials to obtain carbonaceous solid waste (selected material A) and non-carbonaceous solid waste (selected material B).
[0117] (3) mixing the selected material A obtained by sorting in step (2) and the waste electrolyte and carbon slag produced by aluminum electrolysis at a mass ratio of 1:2:2 for 0.5 h to obtain a first mixture; and finely grinding the first mixture to a particle size of 0.1 mm;
[0118] The first mixture after fine grinding is floated: the mixture is added into water, placed in a flotation tank, the speed of the flotation machine is adjusted to be stable, and then stirred in air to make the slurry fully mixed, and then the inhibitor, collector and frother are added in sequence, the scraper speed is controlled, and the aeration volume is adjusted before flotation to obtain waste electrolyte (flotation material C) and carbon powder (flotation material D). Among them, the ore pulp concentration is 25%, the speed of the flotation machine is 2000rpm, and the aeration volume of the flotation machine is selected to be 250L / min. Among them, the inhibitor is selected from water glass; the collector is selected from gasoline and kerosene (the mass ratio of gasoline to kerosene is 1:2); the frother is selected from No. 2 oil.
[0119] (4) drying the flotation material C obtained in step (3) and mixing it with a composite activator at a mass ratio of 1:0.5, placing it in a crucible after mixing for 0.5 hours, and performing medium-temperature activation treatment in a heating furnace. After the reaction is completed, filtering is performed, and the filter residue is dried to obtain aluminum fluoride, and the filtrate is dried at 110° C. to obtain sodium salt. The temperature of the medium-temperature activation treatment is 550° C., and the reaction time is 0.5 hours; the composite activator is selected from aluminum sulfate and sodium aluminate (the mass ratio of aluminum sulfate to sodium aluminate is 1:0.5).
[0120] (5) The flotation material D obtained in step (3) is first dried in an air-tight environment at a temperature of 120° C. for 1 h, and then the temperature is raised to 450° C. for carbonization for 1 h; after the carbonization is completed, an activation gas is introduced for activation treatment, the temperature is controlled at 750° C., and the activation gas is air; after the activation is completed, the activated material is cooled with circulating water to obtain activated carbon.
[0121] (6) Finely grind the selected material B obtained in step (2) to a particle size of about 1.5 mm, mix the finely ground powder with activated carbon in a mass ratio of 1:0.4, add the powder into water and stir for hydration treatment, the water temperature is 40°C, and the stirring time is 0.5 h; after hydration treatment, filter and dry to obtain a refractory raw material.
[0122] Example 5
[0123] (1) The overhaul slag is placed in a crusher for coarse crushing to obtain overhaul slag with a particle size of 5 mm.
[0124] (2) The overhaul slag after crushing and screening is automatically sorted by a color sorter according to the color difference of different materials to obtain carbonaceous solid waste (selected material A) and non-carbonaceous solid waste (selected material B).
[0125] (3) mixing the selected material A obtained by sorting in step (2) and the waste electrolyte and carbon slag produced by aluminum electrolysis at a mass ratio of 1:2:2 for 0.5 h to obtain a first mixture; and finely grinding the first mixture to a particle size of 0.1 mm;
[0126] The first mixture after fine grinding is floated: the mixture is added into water, placed in a flotation tank, the speed of the flotation machine is adjusted to be stable, and then stirred in air to make the slurry fully mixed, and then the inhibitor, collector and frother are added in sequence, the scraper speed is controlled, and the aeration volume is adjusted before flotation to obtain waste electrolyte (flotation material C) and carbon powder (flotation material D). Among them, the ore pulp concentration is 35%, the speed of the flotation machine is 3000rpm, and the aeration volume of the flotation machine is selected to be 350L / min. Among them, the inhibitor is selected from water glass; the collector is selected from gasoline and kerosene (the mass ratio of gasoline to kerosene is 1:2); the frother is selected from No. 2 oil.
[0127] (4) drying the flotation material C obtained in step (3) and mixing it with a composite activator at a mass ratio of 1:0.3, placing it in a crucible after mixing for 0.5 h, and performing medium-temperature activation treatment in a heating furnace. After the reaction is completed, filtering is performed, and the filter residue is dried to obtain aluminum fluoride, and the filtrate is dried at 110° C. to obtain sodium salt. The temperature of the medium-temperature activation treatment is 450° C., and the reaction time is 0.5 h; the composite activator is selected from aluminum sulfate and sodium aluminate (the mass ratio of aluminum sulfate to sodium aluminate is 1:0.5).
[0128] (5) The flotation material D obtained in step (3) is first dried in an air-tight environment at a temperature of 120° C. for 0.5 h, and then the temperature is raised to 600° C. for carbonization for 0.5 h; after the carbonization is completed, an activation gas is introduced for activation treatment, the temperature is controlled at 900° C., and the activation gas is air; after the activation is completed, the activated material is cooled with circulating water to obtain activated carbon.
[0129] (6) Finely grind the selected material B obtained in step (2) to a particle size of about 1.5 mm, mix the finely ground powder with activated carbon in a mass ratio of 1:0.5, add the mixture into water and stir for hydration treatment, the water temperature is 50°C, and the stirring time is 0.5 h; after hydration treatment, filter and dry to obtain a refractory raw material.
[0130] Embodiment 6:
[0131] The invention is basically the same as Example 1, except that the inhibitor is selected from water glass; the capture agent is selected from gasoline and light diesel oil (the mass ratio of gasoline and light diesel oil is 1:2); the foaming agent is selected from No. 2 oil; and the composite activator is selected from aluminum carbonate and potassium aluminate (the mass ratio of aluminum carbonate and potassium aluminate is 1:0.5).
[0132] Example 7
[0133] The invention is basically the same as Example 1, except that the inhibitor is selected from water glass; the capture agent is selected from light diesel oil and kerosene (the mass ratio of light diesel oil and kerosene is 1:2); the foaming agent is selected from No. 2 oil; and the composite activator is selected from aluminum sulfate, aluminum nitrate and sodium aluminate (the mass ratio of aluminum sulfate, aluminum nitrate and sodium aluminate is 1:0.5:0.5).
[0134] The processing parameters of Examples 1 to 7 are shown in Table 1.
[0135] Table 1
[0136]
[0137] Performance Testing
[0138] (1) The chemical composition of the aluminum fluoride produced in the above Examples 1 to 7 was tested and analyzed respectively, and the ignition loss of aluminum fluoride at 550° C. was tested with reference to GB / T 4292-2017 and YS / T 581. The results are shown in Table 2.
[0139] Table 2
[0140]
[0141] (2) The iodine adsorption value, methylene blue adsorption value and chemical oxygen demand removal rate of the activated carbon produced in Examples 1 to 7 were tested respectively. The iodine adsorption value, methylene blue adsorption value and chemical oxygen demand removal rate were tested with reference to GB / T 1249.1-1999 standard, and the test results are shown in Table 3.
[0142] Table 3
[0143]
[0144] (3) The components of the refractory raw materials produced in the above Examples 1 to 7 were tested respectively. The test results are shown in Table 4.
[0145] Table 4
[0146]
[0147] It can be seen from the above table that the treatment method of the present application can effectively convert the solid waste generated in the electrolytic aluminum production process into aluminum fluoride, activated carbon and refractory raw materials; compared with Examples 2 to 3, the performance parameters in Examples 1 and 4 to 7 are all within the optimal range, and the aluminum fluoride finally prepared has a lower loss on ignition, and the iodine adsorption value and methylene blue adsorption value of the activated carbon and the chemical oxygen demand removal rate are all higher.
[0148] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0149] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A method for treating solid waste from aluminum electrolysis, characterized in that: The steps include: Providing aluminum electrolysis solid waste, wherein the aluminum electrolysis solid waste includes aluminum waste electrolyte, carbon slag and overhaul slag; The overhaul slag is subjected to coarse grinding and sorting treatment in sequence to obtain non-carbonaceous solid waste and carbonaceous solid waste; Mixing the carbonaceous solid waste, the waste aluminum electrolyte and the carbon slag to obtain a first mixture; performing flotation treatment on the first mixture to obtain spent electrolyte and carbon powder; The waste electrolyte and the composite activator are mixed, and medium-temperature activation treatment and filtration treatment are performed in sequence to obtain aluminum fluoride and a filtrate.
2. The method for treating solid waste from aluminum electrolysis according to claim 1, characterized in that: The treatment method further comprises the following steps: sequentially performing carbonization treatment and activation treatment on the carbon powder to obtain activated carbon; Optionally, the temperature of the carbonization treatment is 300° C. to 600° C., and the time of the carbonization treatment is 0.5 h to 1.5 h; Optionally, the activation treatment temperature is 600° C. to 900° C.; Optionally, the activation gas for the activation treatment is selected from one or more of water vapor, carbon dioxide and air.
3. The method for treating solid waste from aluminum electrolysis according to claim 2, characterized in that: The treatment method further comprises the following steps: grinding the non-carbonaceous solid waste to a particle size of 0.5 mm to 1.5 mm, mixing the non-carbonaceous solid waste with the activated carbon, and sequentially performing hydration treatment, filtering treatment and drying treatment to obtain a refractory material raw material; Optionally, the hydration treatment time is 0.5h~1.5h; Optionally, the mixing mass ratio of the non-carbonaceous solid waste to the activated carbon is 1:(0.3-0.5); Optionally, the water temperature in the hydration treatment is 30°C~50°C.
4. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The treatment method further comprises the following steps: drying the filtrate to obtain sodium salt.
5. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The mass ratio of the carbonaceous solid waste, the waste aluminum electrolyte and the carbon slag is 1:(2-3):(2-3).
6. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The mass ratio of the waste electrolyte to the composite activator is 1:(0.3-0.7).
7. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: Before flotation of the first mixture, the method further comprises the following steps: fine grinding the first mixture to a particle size of 0.04 mm to 0.1 mm.
8. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The composite activator is selected from two or more of aluminum sulfate, aluminum nitrate, aluminum carbonate, aluminum chloride, sodium aluminate and sodium aluminate.
9. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The temperature of the medium-temperature activation treatment is 450° C. to 650° C.; the time of the medium-temperature activation treatment is 0.5 h to 1.5 h.
10. The method for treating solid waste from aluminum electrolysis according to any one of claims 1 to 3, characterized in that: The processing method meets at least one of the following conditions: (1) The pulp concentration in the flotation process is 15wt%~35wt%; the rotation speed of the flotation process is 1000rpm~3000rpm; the aeration volume of the flotation process is 150L / min~350L / min; (2) The inhibitor of the flotation treatment is selected from one or more of lime, sodium carbonate and water glass; (3) the collector used in the flotation treatment is selected from one or more of light diesel, kerosene and gasoline; and (4) The frother used in the flotation treatment is selected from one or more of No. 2 oil, eucalyptus oil and camphor oil.