Method for extracting lead and iodine from waste lead-based perovskite battery to prepare lead iodide
Through ultrasonic water immersion and pH adjustment methods, the problem of using toxic organic solvents in the prior art was solved, and efficient and environmentally friendly extraction of lead and iodine was achieved, leading recovery rate and purity of lead iodide were improved, and lead iodide was simplified. Process flow.
Patent Information
- Application Number
- CN202410976986.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Prior art When extracting lead and iodine from waste lead-based perovskite batteries, toxic organic solvents are widely used, resulting in environmental and health threats, and the process is complex and not environmentally friendly.
Ultrasonic water immersion method is used to separate the substrate and back plate of the waste lead-based perovskite battery, use water as a solvent, and achieve efficient extraction of lead iodide by adjusting the pH value and incomplete evaporation of crystallization, avoiding the use of toxic organic solvents .
The lead extraction rate of more than 99.9% was achieved, which avoided the harm of toxic solvents to the environment and the human body, improved the purity of lead iodide and the environmental protection of the process, and simplified the subsequent separation and purification operations.
Smart Images

Figure CN118929737A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of waste perovskite battery recycling, and specifically relates to a method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide, and in particular to a method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide by ultrasonic water leaching. Background Art
[0002] Lead-based perovskite cells have shown great commercial prospects due to their advantages of high photoelectric conversion efficiency and low manufacturing cost. With the accelerated upgrading of the industry and the replacement of products, a large number of unqualified or retired lead-based perovskite cells eliminated from the production line are facing the problem of disposal, especially the environmental risks brought by the lead-containing materials used in the perovskite layer have attracted much attention. Based on the comprehensive consideration of environmental protection and resource utilization, it is crucial to develop effective lead pollution control and lead-based perovskite cell recycling technology.
[0003] Extracting lead and iodine from lead-based perovskite batteries can be done by wet separation and recovery. First, the perovskite layer needs to be stripped from the discarded battery panel, and then lead is recovered from it by adsorption, electrolysis, precipitation and other means, and further processed to obtain lead iodide or refined lead products. There are some technical solutions for recovering lead in the field, but there are still defects.
[0004] Patent CN114988464A discloses a method and device for recycling lead salts from perovskite batteries, including leaching the perovskite battery with an organic reagent, then adding deionized water and glacial acetic acid to the perovskite battery leaching solution to obtain a suspension, heating the suspension in a water bath until all the orange-yellow precipitates settle to the bottom, washing and drying to obtain purified lead iodide crystals. The leaching agents used include toxic organic solvents such as DMF, DMSO, GBL, and 2-ME, which will inevitably evaporate into the environment and cause harm during the water bath heating of the suspension.
[0005] Patent CN107513618B discloses a method and device for recovering lead from perovskite batteries, comprising crushing the perovskite battery to obtain lead 3 The crushing operation significantly reduces the recycling value of the substrate and backplane, and the remaining organic solution is not effectively utilized, which poses environmental risks and hidden dangers.
[0006] Patent CN108823414B discloses a method for recycling waste perovskite solar cells, wherein the perovskite solar cell is immersed in an organic solvent for cleaning, and a lead-containing leaching solution is obtained after solid-liquid separation, and the obtained lead-containing leaching solution is reacted with ammonia water, and the obtained first turbid liquid is solid-liquid separated to obtain a first solid, and the obtained first solid is reacted with acetic acid, and the obtained second turbid liquid is solid-liquid separated to obtain lead acetate solid. The process flow is cumbersome and lengthy, and the waste liquid generated is not effectively treated.
[0007] In summary, current research related to the recycling of waste lead-based perovskite batteries basically requires the use of organic solvents (such as DMF, DMSO, etc.) to achieve the dissolution and separation of the perovskite layer. However, the large-scale use of toxic organic solvents poses a direct threat to the operating environment and personnel health. It is urgent to develop new methods for lead separation and recovery based on green reagents. Summary of the invention
[0008] In response to the need for improvement in the prior art, the present invention provides a method for extracting lead and iodine from discarded lead-based perovskite batteries to prepare lead iodide, which uses an ultrasonic water immersion method, then adjusts the pH to 2.5-5.0, and performs incomplete evaporation crystallization or cooling crystallization on the first solution obtained by filtration to obtain lead iodide. This method solves the problem of secondary pollution caused by toxic organic solvents widely used in the field of wet recovery of existing perovskite batteries.
[0009] According to the purpose of the present invention, there is provided a method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide, comprising the following steps:
[0010] (1) Separating the substrate and back plate of the discarded lead-based perovskite battery to expose the perovskite layer;
[0011] (2) extracting the substrate and back plate separated in step (1) with water and performing ultrasonic treatment;
[0012] (3) removing the substrate and the back plate, adding acid to the extract, adjusting the pH to 2.5-5.0, and then filtering to obtain a first solution;
[0013] (4) subjecting the first solution obtained in step (3) to evaporative crystallization or cooling crystallization, wherein the evaporative crystallization is incomplete evaporative crystallization, i.e., evaporating the volume of the first solution to 2%-10% of the initial volume, and crystallizing to obtain lead iodide.
[0014] Preferably, in step (4), the solution remaining after crystallization is recorded as the second solution, and the second solution is reused in step (3) to adjust the pH of the next batch.
[0015] Preferably, in step (3), the acid is hydroiodic acid, hydrochloric acid, hydrobromic acid, acetic acid or nitric acid.
[0016] Preferably, in step (2), the power density of the ultrasound is 0.3-2 W / cm 2 The frequency of ultrasound is 20-100kHz; the temperature of water extraction is 10-40°C, and the time is 10-60min.
[0017] Preferably, in step (2), the ratio of the volume of water used for water extraction to the area of a single surface of the waste lead-based perovskite battery is 5-20 L / m 2 .
[0018] Preferably, the material of the perovskite layer is an APbI3 type structure, and the A-position cation is Cs + 、MA + , FA + one or a mixture of them.
[0019] Preferably, in step (1), the separation method is mechanical cutting, and / or immersing the discarded lead-based perovskite battery in a non-polar solvent to render the encapsulation film ineffective.
[0020] Preferably, the packaging film is a polyolefin elastomer or a polyethylene-polyvinyl acetate copolymer.
[0021] Preferably, the non-polar solvent is one of n-hexane, cyclohexane and toluene.
[0022] Preferably, the cooling crystallization is to reduce the temperature of the first solution to 0-4°C.
[0023] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0024] (1) In response to the defects or improvement needs of the prior art, the present invention does not use toxic organic solvents such as DMF, DMSO, γ-GBL, NMP, etc. in the process of dissolving the perovskite layer to extract lead. Instead, green, harmless, cheap and easily available water is used as a solvent, assisted by ultrasound, which can achieve a lead extraction rate of more than 99.9% (lead extraction rate = lead content in the extract / lead content in the discarded lead-based perovskite battery × 100%). Not only can it efficiently recover lead from discarded lead-based perovskite batteries, but it can also avoid the harm of toxic organic solvents to the environment and human body. Using water as a solvent to dissolve the perovskite layer and extract lead will not cause damage to other functional layers (such as the electron transport layer SnO2, the hole transport layer NiO x ) to avoid the introduction of metallic impurity elements into the leaching solution, so that the leaching solution only contains perovskite-related components, which greatly simplifies the subsequent separation and purification operations, and the lead iodide product has high purity.
[0025] (2) To extract lead from discarded lead-based perovskite batteries, the perovskite layer needs to be exposed. The POE or EVA packaging films widely used in the field of photovoltaic packaging have strong adhesion, and the substrate and the backplane are difficult to separate. The present invention mechanically cuts or soaks the discarded lead-based perovskite batteries in a non-polar solvent, and the non-polar solvent is one of n-hexane, cyclohexane, and toluene. According to the principle of "like dissolves like", they can spontaneously penetrate into the packaging layer and reduce the viscosity between the packaging film and the interface of the surrounding materials. In addition, n-hexane, cyclohexane, and toluene will not destroy the perovskite layer, thereby avoiding Pb leakage. The properties of the used non-polar solvent have not changed, and it can be recycled for the separation process of the substrate and the backplane of the next batch.
[0026] (3) The present invention adds hydroiodic acid to the leaching solution to adjust the pH to 2.5-5.0, inhibits the formation of lead iodide hydrolysis product Pb(OH)I, prevents lead from being discharged from the system in the form of Pb(OH)I filter residue in the subsequent filtration operation, and causes a decrease in the lead recovery rate; at the same time, adding hydroiodic acid to the first solution can also prevent the generation of Pb(OH)I impurities during the crystallization process, further improving the purity of the lead iodide product. In addition, the present invention requires that hydroiodic acid be added after the substrate and the back plate are removed to avoid the acidic environment from dissolving the remaining metal element functional layer on the substrate and the back plate, and to prevent the introduction of metal element impurities into the leaching solution, thereby creating favorable conditions for preparing high-purity lead iodide.
[0027] (4) The present invention adopts an incomplete evaporation method, specifically, the volume of the first solution is evaporated to 2%-10% of the initial volume, so that the lead iodide crystals are precipitated first, and the Cs contained in the first solution is avoided. + 、MA + , FA + The A-site cations of the perovskite enter the lead iodide product to form an impurity phase, thereby improving the purity of the lead iodide product.
[0028] (5) The present invention constructs a process for recycling reagents. Specifically, the non-polar solvent can be recycled and reused in the next batch of double-glass separation process; the second solution remaining after crystallization can be reused in the next batch of pH adjustment process. The discharge of waste liquid is avoided, environmental hazards are reduced, and process economy is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a process flow chart of the present invention.
[0030] Figure 2 Optical photographs and SEM images of the substrate surface before and after ultrasonic water immersion.
[0031] Figure 3 The SEM image of the substrate surface after water immersion without ultrasonic treatment.
[0032] Figure 4 This is the dominant area diagram of Pb element in water (c(Pb)=0.001mol / L).
[0033] Figure 5 XRD patterns of incomplete evaporation products under pH adjustment and without pH adjustment.
[0034] Figure 6 XRD patterns of the products obtained under incomplete evaporation and complete evaporation after pH adjustment.
[0035] Figure 7 This is the SEM image of the product obtained under incomplete evaporation conditions after pH adjustment. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0037] Reference Figure 1 The present invention provides a method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide. The method comprises:
[0038] (1) Separating the substrate and back plate of the discarded lead-based perovskite battery to expose the perovskite layer;
[0039] (2) extracting the substrate and back plate separated in step (1) with water and performing ultrasonic treatment;
[0040] (3) removing the substrate and the back plate, adding acid to the extract, adjusting the pH to 2.5-5.0, and then filtering to obtain a first solution;
[0041] (4) subjecting the first solution obtained in step (3) to evaporative crystallization or cooling crystallization, wherein the evaporative crystallization is incomplete evaporative crystallization, i.e., evaporating the volume of the first solution to 2%-10% of the initial volume, and crystallizing to obtain lead iodide.
[0042] The substrate and backplane of the discarded perovskite battery are firmly bonded under the action of the photovoltaic adhesive film and are not easy to separate. The present invention exposes the perovskite layer by mechanically cutting and separating the substrate and backplane, or soaking the discarded lead-based perovskite battery with a non-polar solvent such as n-hexane, cyclohexane, and toluene. The non-polar solvent will spontaneously penetrate into the interior of the component to balance the internal and external air pressures, weaken the capillary adhesion, promote the separation of the substrate and the backplane, and expose the middle perovskite layer for subsequent leaching.
[0043] Highly polarized water molecules can form strong hydrogen bonds with the A-site cations of the perovskite, destroying the bond between the A-site cations and [PbI6] 4- The connection between the octahedra causes the collapse of the perovskite crystal structure. As shown in formulas (1)-(2), the decomposition products of methylamine lead iodine include PbI2 and CH3NH3I when it comes into contact with water. Water can further protonate CH3NH3I to generate CH3NH2 and HI. Other types of perovskite materials such as formamidinium lead iodine (FAPbI3) and cesium lead iodine (CsPbI3) will undergo similar decomposition processes when they come into contact with water.
[0044]
[0045] CH3NH3I(aq) → CH3NH2(aq) + HI(aq) (2)
[0046] Therefore, the present invention proposes to use water as a leaching solvent to decompose the exposed perovskite layer material. The lead content in the discarded lead-based perovskite battery is generally 0.5-1.2g / m 2 , converted into lead iodide is 1.1-2.7g / m 2 The solubility of lead iodide in water increases with temperature, specifically 44 mg (0°C), 56 mg (10°C), 69 mg (20°C), 90 mg (30°C), and 124 mg (40°C). Preferably, the ratio of the amount of water used in the cleaning step of the present invention to the area of a single surface of the waste lead-based perovskite battery is 5-20 L / m 2 The reaction temperature is 10-40°C, which can ensure that the lead iodide produced by the decomposition of perovskite can be completely dissolved in water. In addition, ultrasound can accelerate the dissolution and shedding of perovskite and lead-containing phases, further improving the lead extraction rate. As a preferred method, the ultrasonic power density is 0.3-2W / cm 2 , the ultrasonic frequency is 20-100kHz, and the reaction time is 10-60min. Increasing the amount of water, raising the reaction temperature, increasing the ultrasonic power density and frequency, and extending the reaction time can promote the decomposition of perovskite and the dissolution of lead iodide. From the perspective of saving water and energy consumption, the selection of each parameter should not be too large.
[0047] like Figure 2 As shown in the figure, a layer of perovskite film is deposited on the surface of the original substrate. After ultrasonic water immersion, the surface of the substrate is very clean. The substrate with lead eluted can be treated according to the standards of ordinary construction waste, avoiding the expensive treatment costs of discarded perovskite components as hazardous waste. Figure 3 As shown, when ultrasonic treatment is not adopted, a large amount of lead particles still remain on the surface of the substrate, and the effect is not good.
[0048] The leaching solution contains a small amount of debris that falls off from the discarded perovskite battery, and filtering can prevent the subsequent crystallization product from containing impurities. However, lead iodide will undergo a hydrolysis reaction shown in formula (3) in a humid environment to produce Pb(OH)I.
[0049]
[0050] Compared with PbI2, Pb(OH)I is insoluble in water and will be discharged together with debris and dust mixed with discarded perovskite batteries during filtration, reducing the yield of lead iodide. In order to inhibit the formation of Pb(OH)I, the present invention adds acid to the first solution to reverse the above reaction. Taking the addition of HI as an example, Figure 4 The dominant region of Pb in an aqueous solution with a Pb concentration of 1 mmol / L. - The concentration is 10 -3 -10 -2.4 mol / L (i.e. 1-4mmol / L), the Pb element is mainly in the form of Pb 2+ In the form of increasing pH or increasing I - Concentration will produce Pb(OH)2 or PbI2 precipitation, which will be discharged from the system during filtration, resulting in a large lead loss rate (lead loss rate = (1-lead content in the first solution / lead content in the extract) × 100%). HI is a strong acid and is completely ionized in water. + Concentration and I - The concentrations are almost equal, and the pH decrease is accompanied by I - When the concentration increases and the pH is too low, I - Increased concentration will lead to the precipitation of PbI2. Therefore, the present invention limits the amount of acid added to a concentration of no more than 10 -2.4 mol / L, so the pH needs to be greater than 2.4, and the pH range is 2.5-5.0. At this time, Pb in the solution mainly exists in the form of ions, which inhibits the formation of Pb(OH)2, Pb(OH)I and PbI2, and the lead loss rate in the filtration step is low.
[0051] The substrate and backplane contain conductive indium tin oxide, SnO2 as an electron transport layer, and NiO as a hole transport layer. x In order to prevent the above metal elements from dissolving into the leaching solution to form impurities in an acidic environment, the present invention first takes the substrate and the back plate out of the leaching solution and then adds acid into the leaching solution.
[0052] Adjusting the pH value can not only reduce the lead loss during the filtration process, but also prevent the generation of Pb(OH)I by-product during the crystallization process. Figure 5The XRD patterns of the incomplete evaporation crystallization products under the conditions of pH adjustment and non-pH adjustment. In addition to PbI2, the diffraction peak of Pb(OH)I was also detected in the product without pH adjustment. After pH adjustment, only the diffraction peak of PbI2 was detected in the product, and the purity was higher.
[0053] The present invention adopts incomplete evaporation means. Preferably, the incomplete evaporation is to reduce the volume of the first solution to 2%-10% of the initial volume by evaporation. Figure 6 The XRD patterns of the crystals precipitated under incomplete evaporation and complete evaporation are shown in Figure 2. The diffraction peaks of the incomplete evaporation product are basically consistent with the PbI2 standard PDF card, while the complete evaporation product contains impurity peaks. x MA y FA 1-x-y Taking PbI3 ternary cationic perovskite as an example, the first solution contains Cs + 、MA + , FA + , Pb 2+ ,I - Ions, PbI2 is slightly soluble in water, while CsI, MAI, and FAI are all easily soluble in water. Therefore, PbI2 is precipitated first during evaporation, and the solid product recovered at this time has high purity, while the solid product obtained by complete evaporation contains impurities formed by the combination of multiple ions.
[0054] In summary, after adjusting the pH of the leaching solution and incompletely evaporating the first solution, a high-purity lead iodide product can be obtained. The SEM image and EDS surface scanning element quantitative results are as follows: Figure 7 As shown, the morphology is regular, and lead and iodine are evenly distributed, which conforms to the atomic ratio characteristic of 1:2.
[0055] The remaining small amount of the second solution that has not been evaporated contains the added acid and a small amount of Pb 2+ ,I - , which can be reused in the pH adjustment process of the next batch, and no waste liquid is discharged during the whole process.
[0056] The following is a specific implementation method
[0057] Example 1
[0058] 1m 2 A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 5L water for 60 minutes at a temperature of 40°C and an ultrasonic power density of 2W / cm 2, the frequency is 100kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 139.97mg / L, 0.011mg / L, 0.007mg / L, 0.002mg / L, and 0.004mg / L, respectively, and the Pb extraction rate in the water washing process is 99.98%. Take out the substrate and the back plate, add hydroiodic acid to the leaching solution, adjust the pH to 2.5, filter and remove suspended particles to obtain the first solution, whose Pb concentration is 133.62mg / L, and the Pb loss rate in the filtration process is 4.54%. The first solution is placed at 60°C and evaporated until 100mL remains, 1434.0mg of lead iodide product is precipitated, the Pb recovery rate in the crystallization step is 96.47%, and no In, Sn, Cu, and Ni impurities are detected in the lead iodide. The remaining 100mL of the second solution is reused in the pH adjustment process of the next batch.
[0059] Example 2
[0060] 0.5m 2 A discarded lead-based perovskite battery containing 500 mg of lead was immersed in cyclohexane for 4 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 10L water for 30 minutes at a temperature of 30°C and an ultrasonic power density of 1.5W / cm 2 , the frequency is 70kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 49.98 mg / L, 0.007 mg / L, 0.004 mg / L, 0.001 mg / L, and 0.002 mg / L, respectively, and the Pb extraction rate in the water washing process is 99.96%. Take out the substrate and the back plate, add nitric acid to the leaching solution, adjust the pH to 3.5, filter and remove suspended particles to obtain the first solution, whose Pb concentration is 47.87 mg / L, and the Pb loss rate in the filtration process is 4.23%. The first solution is placed at 70°C and evaporated until 1L remains, 974.0 mg of lead iodide product is precipitated, the Pb recovery rate in the crystallization step is 91.45%, and no In, Sn, Cu, and Ni impurities are detected in the lead iodide. The remaining 1L of the second solution is reused in the pH adjustment process of the next batch.
[0061] Example 3
[0062] 2m 2 A discarded lead-based perovskite battery containing 2200 mg of lead was immersed in toluene for 8 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 30L water for 20 minutes at a temperature of 20°C and an ultrasonic power density of 0.8W / cm 2, the frequency is 40kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 73.28mg / L, 0.005mg / L, 0.009mg / L, 0.003mg / L, and 0.004mg / L, respectively, and the Pb extraction rate in the water washing process is 99.93%. Take out the substrate and the back plate, add acetic acid to the leaching solution, adjust the pH to 4.0, filter and remove suspended particles to obtain a first solution with a Pb concentration of 70.04mg / L, and a Pb loss rate of 4.42% during the filtration process. The first solution was evaporated at 40°C until 1.5L remained, and 4428.9mg of lead iodide product was precipitated. The Pb recovery rate in the crystallization step was 94.74%, and no In, Sn, Cu, or Ni impurities were detected in the lead iodide. The remaining 1.5L of the second solution was reused for the pH adjustment process of the next batch.
[0063] Example 4
[0064] 1m 2 The discarded lead-based perovskite battery containing 900 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 8L of water for 10 minutes at a temperature of 10°C and an ultrasonic power density of 0.3W / cm 2 , the frequency is 20kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 112.40 mg / L, 0.010 mg / L, 0.006 mg / L, 0.003 mg / L, and 0.001 mg / L, respectively, and the Pb extraction rate in the water washing process is 99.91%. Take out the substrate and the back plate, add hydrochloric acid to the leaching solution, adjust the pH to 5.0, filter and remove the suspended particles to obtain the first solution, whose Pb concentration is 106.86 mg / L, and the Pb loss rate in the filtration process is 4.93%. The first solution is cooled to 0°C, and 1609.8 mg of lead iodide product is precipitated. The Pb recovery rate in the crystallization step is 84.64%, and no In, Sn, Cu, and Ni impurities are detected in the lead iodide. The remaining second solution after cooling and crystallization can be reused in the pH adjustment process of the next batch.
[0065] Comparative Example 1
[0066] The difference between this embodiment and embodiment 1 is that the extraction process is not assisted by ultrasound, and specifically includes the following steps:
[0067] 1m 2A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and the backplane. The substrate and the backplane were statically immersed in 5L of water for 60 minutes at a temperature of 40°C. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution were 123.80 mg / L, 0.011 mg / L, 0.007 mg / L, 0.002 mg / L, and 0.004 mg / L, respectively, and the Pb leaching rate during the water washing process was 88.43%.
[0068] Obviously, the Pb extraction rate decreased significantly without ultrasound. Figure 3 As shown in the figure, a large amount of lead particles still remain on the surface of the substrate, and the Pb removal effect is poor.
[0069] Comparative Example 2
[0070] The difference between this embodiment and embodiment 1 is that DMF is selected as the leaching solvent of the perovskite layer, and specifically includes the following steps:
[0071] 1m 2 A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 5L DMF for 60 minutes at a temperature of 40°C and an ultrasonic power density of 2W / cm 2 , the frequency is 100kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 139.97mg / L, 1.15mg / L, 1.89mg / L, 0.74mg / L, and 0.55mg / L, respectively, and the Pb extraction rate in the cleaning process is 99.98%. Take out the substrate and back plate, filter to remove the suspended particles, and obtain the first solution. The first solution was evaporated at 60°C until 5mL remained, and 16.7mg of lead iodide product was precipitated. The Pb recovery rate in the crystallization step was only 1.07%, and the In, Sn, Cu, and Ni content in lead iodide were 23mg / kg, 26mg / kg, 18mg / kg, and 15mg / kg, respectively.
[0072] It can be seen that when DMF is used as the leaching solvent, other functional layers in the perovskite battery will dissolve in small amounts, and the concentration of metal impurities in the leaching solution will increase, which will lead to more metal impurities mixed in the lead iodide product. In addition, since the solubility of PbI2 in DMF is much higher than that in water, even if it is evaporated to 0.1% (5mL) of the original volume (5L), it is difficult to precipitate lead iodide crystals, and the lead recovery rate is extremely low. If a complete evaporation operation is adopted, the product will be mixed with impurities such as Cs, MA, FA, and it will be impossible to obtain lead iodide. Figure 6 shown.
[0073] Comparative Example 3
[0074] The difference between this embodiment and embodiment 1 is that no hydroiodic acid is added to adjust the pH, and the present embodiment specifically comprises the following steps:
[0075] 1m 2 A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 5L water for 60 minutes at a temperature of 40°C and an ultrasonic power density of 2W / cm 2 , the frequency is 100kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 139.97mg / L, 0.011mg / L, 0.007mg / L, 0.002mg / L, and 0.004mg / L, respectively, and the Pb extraction rate in the water washing process is 99.98%. The substrate and back plate are taken out, and the suspended particles are filtered to obtain the first solution, whose Pb concentration is 124.70mg / L, and the Pb loss rate in the filtration process is 10.91%.
[0076] Obviously, due to the absence of hydroiodic acid, a small amount of insoluble Pb(OH)I was present in the leaching solution, which was discharged as filter residue during filtration. The Pb loss rate (10.91%) was significantly higher than the value (4.54%) under pH adjustment in Example 1.
[0077] The first solution was evaporated at 60°C until 100 mL remained, and 1274.8 mg of solid was precipitated. No In, Sn, Cu, or Ni impurities were detected. XRD analysis of the product showed the following results: Figure 5 As shown, the main phase is PbI2, and it also contains a small amount of Pb(OH)I phase, and the product is impure.
[0078] Comparative Example 4
[0079] The difference between this embodiment and embodiment 1 is that a solid product is obtained by complete evaporation, which specifically includes the following steps:
[0080] 1m 2 A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 5L water for 60 minutes at a temperature of 40°C and an ultrasonic power density of 2W / cm 2, the frequency is 100kHz. The concentrations of Pb, In, Sn, Cu, and Ni in the leaching solution are 139.97 mg / L, 0.15 mg / L, 0.17 mg / L, 0.09 mg / L, and 0.05 mg / L, respectively, and the Pb extraction rate in the water washing process is 99.98%. Take out the substrate and the back plate, add hydroiodic acid to the leaching solution, adjust the pH to 2.5, filter to remove suspended particles, and obtain a first solution with a Pb concentration of 133.62 mg / L. The Pb loss rate in the filtration process is 4.54%. The first solution was completely evaporated at 60°C, and 1844.3 mg of solid was precipitated. The product was subjected to XRD analysis, and the results are as follows Figure 6 As shown, the product contains not only PbI2 but also unidentified impurities, which does not meet the target requirement of preparing PbI2.
[0081] Comparative Example 5
[0082] The difference between this embodiment and embodiment 1 is that the 2 The water consumption includes the following steps:
[0083] 1m 2 A discarded lead-based perovskite battery containing 700 mg of lead was immersed in n-hexane for 2 hours to separate the substrate and backplane. The substrate and backplane were ultrasonically cleaned in 2L of water for 60 minutes at a temperature of 40°C and an ultrasonic power density of 2W / cm 2 , the frequency is 100kHz. The concentrations of Pb, In, Sn, Cu and Ni in the leaching solution are 290.40mg / L, 0.025mg / L, 0.019mg / L, 0.011mg / L and 0.008mg / L respectively, and the Pb leaching rate in the water washing process is 82.97%.
[0084] The water consumption in this case is only 2L / m 2 , it is impossible to fully dissolve the PbI2 produced by the decomposition of the perovskite layer. The undissolved PbI2 remains on the substrate and backplane, and the lead leaching rate is significantly reduced, making it impossible to achieve the harmlessness of discarded lead-based perovskite components.
[0085] If the intake is higher than 20L / m 2 There is no obvious improvement or enhancement on various technical indicators, but the evaporation and crystallization process will consume extra energy, so it is not recommended.
[0086] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide, It is characterized in that The following steps are involved: (1) Separating the substrate and back plate of the discarded lead-based perovskite battery to expose the perovskite layer; (2) extracting the substrate and back plate separated in step (1) with water and performing ultrasonic treatment; (3) removing the substrate and the back plate, adding acid to the extract, adjusting the pH to 2.5-5.0, and then filtering to obtain a first solution; (4) subjecting the first solution obtained in step (3) to evaporative crystallization or cooling crystallization, wherein the evaporative crystallization is incomplete evaporative crystallization, i.e., evaporating the volume of the first solution to 2%-10% of the initial volume, and crystallizing to obtain lead iodide.
2. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that In step (4), the solution remaining after crystallization is recorded as the second solution, and the second solution is reused in step (3) to adjust the pH of the next batch.
3. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that In step (3), the acid is hydroiodic acid, hydrochloric acid, hydrobromic acid, acetic acid or nitric acid.
4. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that In step (2), the power density of the ultrasound is 0.3-2 W / cm 2 The frequency of ultrasound is 20-100kHz; the temperature of water extraction is 10-40°C, and the time is 10-60min.
5. The method for extracting lead and iodine from waste lead-based perovskite batteries to prepare lead iodide according to claim 1, It is characterized in that In step (2), the ratio of the volume of water used for water extraction to the area of a single surface of the waste lead-based perovskite battery is 5-20 L / m 2 .
6. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that The material of the perovskite layer is APbI 3 Type structure, the A-position cation is Cs + 、MA + , FA + one or a mixture of them.
7. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that In step (1), the separation method is mechanical cutting, and / or immersing the discarded lead-based perovskite battery in a non-polar solvent to render the encapsulation film ineffective.
8. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 7, It is characterized in that The packaging film is polyolefin elastomer or polyethylene-polyvinyl acetate copolymer.
9. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 7 or 8, It is characterized in that The non-polar solvent is one of n-hexane, cyclohexane and toluene.
10. The method for preparing lead iodide by extracting lead and iodine from waste lead-based perovskite batteries according to claim 1, It is characterized in that The cooling crystallization is to reduce the temperature of the first solution to 0-4°C.
Citation Information
Cited By
Perovskite solar cell recycling method
WO2026213907A1