Ferrite magnetic bead and preparation method thereof

By using low-permeability air-gap materials and ultra-thick silver internal electrodes, combined with a three-stage sintering process, high-current magnetic beads with high impedance and low DC resistance at specific frequencies have been fabricated, solving problems such as product cracking. These beads are suitable for applications such as audio noise reduction circuits and new energy vehicles.

CN118929768APending Publication Date: 2024-11-12GUANGDONG FENGHUA ADVANCED TECHNOLOGY (HOLDING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411157601.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies struggle to produce high-current magnetic beads with high impedance and low DC resistance at specific frequencies, and conventional processes lead to problems such as product cracking and delamination, failing to meet the high-performance requirements of fields such as new energy vehicles and fast charging for mobile phones.

Method used

Ferrite beads were fabricated using a low-permeability air gap material and an ultra-thick silver inner electrode design, combined with a three-stage sintering process. The air gap material served as a channel for the leakage of magnetic field lines, suppressing magnetic flux saturation. The thickness of the inner electrode was increased to over 80 μm, and the sintering process was optimized to solve the co-firing problem.

Benefits of technology

It achieves high impedance and low DC resistance in the 100-400MHz frequency range, has a high product appearance qualification rate, and possesses high reliability and stability, making it suitable for audio noise reduction circuits and new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929768A_ABST
    Figure CN118929768A_ABST
Patent Text Reader

Abstract

The invention relates to a ferrite magnetic bead and a preparation method thereof, and belongs to the technical field of ferrite magnetic beads. The preparation method of the ferrite magnetic bead provided by the invention comprises the following steps: (1) printing an air gap layer made of a specific material on a ferrite base layer; (2) printing an ultra-thick silver inner electrode and a filling material on the air gap layer to obtain a dielectric layer diaphragm; (3) the dielectric diaphragms are laminated and cut, and then semi-finished magnetic beads are obtained through three-section sintering; and (4) manufacturing an outer electrode on the semi-finished product magnetic bead to obtain the ferrite magnetic bead. The magnetic bead prepared by the preparation method of the ferrite magnetic bead, provided by the invention, has the characteristics of high impedance, excellent current resistance, low direct-current resistance and large current under the specific frequency of 100-400MHz, is relatively high in appearance yield in the production process, can be widely applied to the fields of audio noise reduction lines, adapters, new energy automobiles and the like, and has extremely high application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ferrite beads, and in particular to a ferrite bead and a preparation method thereof. Background Art

[0002] With the rapid development of new energy vehicles, mobile phone fast charging and other fields, the requirements for high current of miniaturized devices have been further improved. At present, super fast charging of 66W and above has become popular in the domestic consumer market. The design scheme is the application of gallium nitride MOS tube with high current audio beads. The bandgap width of gallium nitride MOS tube is large, which means it can withstand higher electric field strength. Under the same voltage, gallium nitride chips can pass a larger current and thus output greater power. To meet the high power requirements of fast charging, the passive components used with it need to meet higher current resistance.

[0003] Audio magnetic beads belong to a special type of high-current magnetic beads, which have high impedance in a specific frequency band, low DC resistance, low load heat generation, excellent bias characteristics and good current shock resistance. These are excellent characteristics that conventional magnetic beads do not have and are difficult to meet.

[0004] In the prior art, in order to improve the current resistance characteristics of magnetic bead products and reduce the DC resistance of the products, on the one hand, the magnetic circuit can be extended by introducing an air gap to suppress magnetic flux saturation; on the other hand, a thick inner electrode design can be used to reduce DC resistance to improve the current resistance characteristics of the magnetic beads. However, the introduction of air gap materials and thick electrode preparation, and the difference in shrinkage when multiple materials are co-fired, will cause cracking, delamination, warping, etc. in the product, which are key issues that need to be solved urgently. At the same time, with the increase in demand for chips used in fast charging and output power, the performance of conventional high-current magnetic beads can no longer meet the needs of all application scenarios, and further upgrading and optimization of product performance is needed.

[0005] Therefore, there is an urgent need to develop a method for preparing high-current magnetic beads with high impedance and low internal resistance at a specific frequency, while optimizing the process and solving problems such as product cracking and stratification caused by co-firing of materials. The method has high technical difficulty and application value. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a ferrite bead and a preparation method thereof. The magnetic beads prepared by the method provided by the present invention can have high impedance in a specific frequency band of 100-400MHz, and have low DC resistance and large current characteristics. At the same time, the product appearance qualification rate of the product manufactured by the method of the present invention is high, and it has high feasibility for mass production. The unique air gap manufacturing method of the product enables the product to have excellent bias characteristics, and it can still maintain high performance, high reliability, and high stability in high-power load application scenarios. It can be widely used in audio noise reduction circuits, adapters, new energy vehicles and other fields, and has extremely high application value.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] In a first aspect, the present invention provides a method for preparing a ferrite bead, characterized in that it comprises the following steps:

[0009] (1) printing an air gap layer on a ferrite base layer; the ferrite base layer is a perforated ferrite diaphragm, and the magnetic permeability of the material of the air gap layer is 0.01-10H / m;

[0010] (2) printing a silver inner electrode and a filling material on the air gap layer to obtain a dielectric layer membrane; the thickness of the silver inner electrode is ≥80 μm;

[0011] (3) stacking and cutting the dielectric diaphragm, and then sintering in three stages to obtain a semi-finished magnetic bead; in the three stages of sintering, the temperature of the first stage is 210-230° C., the temperature of the second stage is 260-280° C., and the temperature of the third stage is 890-910° C.;

[0012] (4) Making external electrodes on the semi-finished magnetic beads to obtain the ferrite magnetic beads.

[0013] The ferrite base layer used in the present invention is a perforated ferrite membrane, and its preparation method is: using a casting process to prepare ferrite slurry and perform perforation treatment. In the preparation method of the present invention, the printing of the air gap layer avoids the perforation of the base membrane to avoid affecting the interlayer electrode conduction effect.

[0014] The present invention adopts a specific air gap material and prints an air gap layer on the above-mentioned ferrite base layer: the air gap material with a magnetic permeability below 10H / m can be well co-fired with the magnetic material, and the air gap material can be used as a magnetic line leakage channel to extend the magnetic circuit and suppress the internal magnetic flux of the product from reaching saturation, so that the product has better bias characteristics and more stable performance during the application load process.

[0015] The higher the magnetic permeability of the air gap material, the stronger the magnetic conductivity, that is, the worse the suppression effect on the increase of the magnetic flux of the magnetic core, and the easier it is for the magnetic flux inside the product to reach saturation; the ideal magnetic permeability of the air gap material = 0, but based on the limitations of the low-temperature co-firing process of laminated products, the air gap material must be able to achieve a good co-firing effect with the magnet material. At this stage, such materials cannot match the low-temperature co-firing process of laminated ferrite products, and the products manufactured have reliability defects.

[0016] At the same time, in order to achieve the goal of low DC resistance and large rated current products, the present invention adopts an ultra-thick square silver inner electrode process, and increases the thickness of the silver inner electrode to more than 80μm through printing, so that the DC resistance of the ferrite bead is ≤35mΩ, or even lower than 20mΩ, and the temperature rise current is ≥4A.

[0017] Compared with conventional products, thick electrodes generate less heat during the load process than thin electrode devices, and the load life has better durability. In the prior art, the thickness of the inner electrode silver is mostly designed to be less than 50μm, and such characteristics are significantly worse than those of the ferrite beads produced by this method.

[0018] In addition, the present invention also adopts a three-stage sintering process technology at a specific temperature. By adjusting the sintering temperature, heating rate and holding time, it can effectively solve the sintering internal cracking and cracking problems caused by the co-firing of multiple materials and thick electrodes, significantly improve product appearance defects and increase the pass rate. The conventional sintering method is continuous heating, which can easily cause the product appearance to be significantly affected and the pass rate to be reduced.

[0019] The ferrite beads produced by the above-mentioned specific method can have an impedance of 1500Ω at a frequency of 100-400MHz, and can reach more than 1000Ω under the condition of an applied current load. At the same time, they have the characteristics of excellent current resistance, low DC resistance, large current and high appearance qualification rate, and have extremely high application value in the preparation of components in the fields of new energy vehicles, mobile phone fast charging, etc.

[0020] Preferably, in step (1), the material of the air gap layer is NiZn ferrite.

[0021] Preferably, in the steps (1) and (2), the ferrite base layer and the filling material contain main ferrite magnetic powder, and the magnetic permeability of the main ferrite magnetic powder is 50-60 H / m.

[0022] The main magnetic powder and the cast film magnetic powder used in the filling material of the present invention are the same magnetic powder, and the magnetic permeability of the main magnetic powder is significantly higher than that of the magnetic powder of the air gap material NiZn ferrite.

[0023] Further preferably, in the step (2), the filling material is prepared by mixing and rolling the main ferrite magnetic powder, a carrier and a solvent to obtain a printing paste, namely the filling material.

[0024] Preferably, in step (2), the printing of the silver inner electrode comprises: printing a silver inner electrode pattern, drying, and then repeatedly printing and drying on the silver inner electrode pattern until the thickness of the silver inner electrode is reached.

[0025] Further preferably, in the step (2), the filling material is printed in an area outside the silver inner electrode to fill the height difference around the silver inner electrode.

[0026] The filling material used in the present invention can compensate for the height difference and improve stacking and cracking: by printing and filling the filling slurry in the area outside the silver inner electrode on the entire ferrite base layer, the diaphragm can be made flat as a whole, thereby solving the problems of wrinkling, silver deformation, sintering cracking, etc. that occur when the thick silver layer diaphragm in the present invention is stacked.

[0027] Preferably, in step (3), the average heating rate of the first sintering stage is 0.8-1.2°C / min; the average heating rate of the second sintering stage is 0.05-0.12°C / min; the average heating rate of the third sintering stage is 0.1-1.5°C / min.

[0028] Further preferably, in the step (3), the first stage sintering is: heating from 40°C to 220°C at an average heating rate of 1°C / min, and then keeping the temperature for 3.5-4.5h;

[0029] The second stage of sintering is: heating from 220°C to 250°C at an average heating rate of 0.1-0.12°C / min, and then heating from 250°C to 270°C at an average heating rate of 0.06-0.07°C / min, and then keeping the temperature for 4.5-5.5h;

[0030] The third stage of sintering is: heating from 270°C to 300°C at an average heating rate of 0.1°C / min, then heating from 300°C to 450°C at an average heating rate of 0.5°C / min, and then heating from 450°C to 900°C at an average heating rate of 1.5°C / min, and keeping warm for 3.5-4.5h.

[0031] As a preferred solution, the process curve of the three-stage sintering is as follows:

[0032] Starting temperature (℃) Time (min) End temperature(℃) 40 180 220 220 240 220 220 270 250 250 300 270 270 300 270 270 300 300 300 300 450 450 300 900 900 240 900

[0033] Preferably, in the step (3), the dielectric diaphragms are stacked and cut to obtain green compacts, and after the green compacts are debinded, three-stage sintering is performed.

[0034] As a preferred solution, the debinding process curve is as follows:

[0035]

[0036]

[0037] After the green bodies are obtained by lamination and cutting, the above-mentioned binder removal process can be used to further improve sintering cracking and increase the appearance qualification rate of the products without affecting other properties of the obtained ferrite beads.

[0038] In a second aspect, the present invention provides ferrite beads prepared by the above-mentioned preparation method of ferrite beads. The ferrite beads prepared by the above-mentioned preparation method have the characteristics of high impedance, excellent current resistance, low DC resistance and large current.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The present invention uses magnetic ferrite powder with low magnetic permeability to prepare the air gap layer. This material can be well co-fired with the magnetic material to suppress the magnetic flux inside the magnet from reaching saturation, thereby greatly improving the bias characteristics of the product;

[0041] (2) The inner electrode design of the present invention adopts an ultra-thick silver inner electrode, which increases the thickness of the inner electrode from the existing 50 μm to more than 80 μm, thereby realizing the preparation of magnetic bead products with low DC resistance and large rated current;

[0042] (3) The present invention solves the sintering internal cracking and cracking problems caused by the co-firing of multiple materials and thick electrodes in ferrite beads by optimizing and controlling the sintering process, improves the product appearance, and significantly improves the qualified rate. In general, the ferrite beads prepared by the method of the present invention have excellent performance, and can still maintain high performance, high reliability, and high stability in high-power load application scenarios. They can be widely used in audio noise reduction circuits, adapters, new energy vehicles and other fields, and have extremely high application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a schematic diagram of printing the air gap layer, the silver inner electrode and the filling material in Example 1;

[0044] Figure 2 The process flow chart of the preparation of ferrite beads in Example 1 is as follows;

[0045] Figure 3 Impedance-frequency curves of magnetic beads without load obtained for Example 1 and Comparative Example 1;

[0046] Figure 4 The temperature rise current result diagram of the magnetic beads obtained in Example 1 and Comparative Examples 1 and 2;

[0047] Figure 5The DC resistance results of the magnetic beads obtained in Example 1 and Comparative Examples 1 and 2 are shown in FIG.

[0048] Figure 6 The impedance-frequency curves of the magnetic beads obtained in Example 1 and Comparative Example 3 under the condition of applied current load;

[0049] Figure 7 This is a comparison chart of the internal sintering effects of the magnetic bead products prepared in Example 1 and Comparative Example 4. DETAILED DESCRIPTION

[0050] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific examples. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0051] Example 1

[0052] An embodiment of a method for preparing ferrite beads of the present invention comprises the following steps:

[0053] (1) A hole is opened on a ferrite diaphragm obtained by a casting process, and an air gap layer with a thickness of 10 μm is printed on the ferrite diaphragm with the hole (avoiding the hole position); the material of the air gap layer is NiZn ferrite material, and its magnetic permeability is 3H / m; the ferrite diaphragm contains a main magnetic powder, and its magnetic permeability is 55H / m; the schematic diagram of the printed air gap layer is as shown in Figure 1 The sub-figure pointed to by the reference numeral 1 in FIG.

[0054] (2) Printing silver inner electrode material → filling material on the air gap layer in sequence to obtain a dielectric layer membrane:

[0055] The silver inner electrode is obtained by printing → drying → printing → drying → printing → drying. The thickness of the silver layer is 85±5μm and the width is 340μm. The schematic diagram of the printed silver inner electrode is shown in Figure 1 The sub-figure pointed to by reference numeral 2 in FIG.

[0056] (3) The filling material is a slurry made by mixing and rolling the main magnetic powder, the carrier and the solvent. The filling material is filled in the area outside the printed silver inner electrode by printing, and the thickness of the silver inner electrode is filled so that the entire membrane is in a flat state; the schematic diagram of the printed filling material is as follows Figure 1 The sub-figure pointed to by reference numeral 3 in FIG.

[0057] (4) The prepared dielectric diaphragms are stacked to obtain blocks, which are then cut into single green pieces. The green pieces are then sintered in three stages to obtain semi-finished magnetic beads. The sintering temperature process curve is shown in Table 1.

[0058] Table 1 Three-stage sintering temperature process curve of Example 1

[0059]

[0060]

[0061] (5) The sintered semi-finished magnetic beads are terminated with silver electrodes, and then electroplated with nickel layers and tin layers to make external electrodes, thereby obtaining the ferrite magnetic beads.

[0062] The schematic diagram of printing the air gap layer, the silver inner electrode and the filling material in this embodiment is shown in FIG. Figure 1 .

[0063] The preparation process flow chart of ferrite beads in this embodiment is as follows: Figure 2 .

[0064] Example 2

[0065] The only difference between Example 2 and Example 1 is that in step (3), before the three-stage sintering, the green body obtained after cutting is first debinded. The temperature process curve of debinding is shown in Table 2 below.

[0066] Table 2 Temperature process curve of debinding in Example 2

[0067] Starting temperature (℃) Time (min) End temperature(℃) 40 30 180 180 240 180 180 30 190 190 300 190 190 30 200 200 300 200

[0068] Comparative Example 1

[0069] The preparation method of the magnetic beads in Comparative Example 1 is different from that in Example 1 only in that the silver inner electrode is obtained by printing → drying, and the silver layer has a thickness of 40 μm and a width of 340 μm; conventional magnetic beads 1 are prepared.

[0070] Comparative Example 2

[0071] The preparation method of the magnetic beads in Comparative Example 1 is different from that in Example 1 only in that the silver inner electrode is obtained by printing → drying → printing → drying, and the silver layer has a thickness of 60 μm and a width of 340 μm; conventional magnetic beads 2 are prepared.

[0072] Comparative Example 3

[0073] The preparation method of the magnetic beads in Comparative Example 3 is different from that in Example 1 only in that the material of the air gap layer is NiZn ferrite material, and its magnetic permeability is 30H / m; conventional magnetic beads 3 are prepared.

[0074] Comparative Example 4

[0075] The only difference between Comparative Example 4 and Example 1 is that non-magnetic NiZn ferrite material is used as the air gap material; conventional magnetic beads 4 are prepared.

[0076] Comparative Example 5

[0077] The preparation method of magnetic beads in Comparative Example 5 is different from that in Example 1 only in that the temperature change process of sintering in step (3) is as shown in Table 3 below.

[0078] Table 3 Sintering temperature process curve of comparative example 3

[0079] Starting temperature (℃) Time (min) End temperature(℃) 40 300 200 200 60 250 250 450 500 500 120 600 600 90 700 700 240 900 900 240 900

[0080] Effect Example 1

[0081] In order to explore the impedance characteristics and bias characteristics of the magnetic beads prepared by the ferrite magnetic bead preparation method provided by the present invention, the magnetic beads prepared in Example 1 and Comparative Examples 1, 2, and 3 were respectively tested as follows:

[0082] a. Using E4982A bridge + 16192A fixture, the test voltage is 50mV, and the impedance-frequency curves of the beads in Example 1 and Comparative Example 1 under no load are obtained. The results are as follows Figure 3 .

[0083] b. The programmable high-voltage power supply IT6724 outputs the specified load current 0, 1A, 2A, 3A, 4A to the product. At the same time, the thermocouple probe is fully in contact with the product surface to record the current value of the magnetic bead products of Example 1 and Comparative Examples 1 and 2 when the temperature rises from room temperature to 40°C. The results are as follows Figure 4 .

[0084] c. Use RM3542A bridge to clamp the electrodes at both ends of the product, and measure the DC resistance Rdc of the magnetic bead products of Example 1 and Comparative Examples 1 and 2. The results are as follows Figure 5 .

[0085] d. Using the E4982A bridge + 16200B + 16192A fixture, the programmable high-voltage power supply IT6724 outputs a specified load current to the product, and derives the load spectrum curve of the key current value (0, 1A, 2A, 3A, 4A), and obtains the impedance-frequency curve of the magnetic beads of Example 1 and Comparative Example 3 under the condition of applied current load. The results are as follows Figure 6 .

[0086] Depend on Figure 3 It can be seen that the preparation method of the present invention uses a thick silver inner electrode layer of ≥80μm, and the obtained ferrite beads have a higher impedance value in the frequency band of several hundred MHz, which can reach more than 1500Ω, which is significantly higher than the conventional magnetic beads 1 obtained by the conventional printing preparation method in Comparative Example 1, and can effectively suppress noise in the frequency band of 100-400MHz.

[0087] Depend on Figure 4 , 5It can be seen that compared with conventional magnetic beads 1 and 2 in comparative examples 1 and 2, the ferrite magnetic beads prepared by the preparation method of the present invention have higher temperature rise current and low DC resistance.

[0088] Depend on Figure 6 It can be seen that under different external current load conditions, the magnetic permeability of the air gap material controlled by the present invention is 0.01-10H / m, and the impedance value of the obtained ferrite beads is still relatively stable and higher than the conventional beads 3 in comparative example 3, especially when the current load is larger, the performance stability advantage of the product of the present invention is more prominent.

[0089] Effect Example 2

[0090] In order to explore the internal sintering effect of the ferrite bead product prepared by the ferrite bead preparation method provided by the present invention, the cross-section of the ferrite bead product after sintering of Example 1 and Comparative Example 4 was observed and compared. The comparison results of the internal sintering effect of the magnetic bead products prepared in Example 1 and Comparative Example 4 are as follows: Figure 7 .

[0091] Depend on Figure 7 It can be seen that the present invention adopts air gap material with a magnetic permeability of 0.01-10H / m, and the obtained ferrite beads can be well co-fired with the magnetic material, and the air gap material can be used as a leakage channel for magnetic lines of force to extend the magnetic circuit; while in Comparative Example 4, conventional magnetic beads 4 are prepared using non-magnetic air gap material, which fails to achieve good co-firing with the overall structure and has reliability defects.

[0092] Effect Example 3

[0093] In order to explore the appearance of the magnetic beads prepared by the ferrite magnetic beads preparation method provided by the present invention, the magnetic beads were mass-produced using the preparation methods of Examples 1, 2 and Comparative Example 5, respectively, and the appearance qualification rates of the five batches of magnetic beads obtained by the six-sided appearance sorting machine in the production position were compared. The results are shown in Table 4.

[0094] The magnetic bead product is qualified if there is no electrode side crack, magnet side crack, or broken corners on the six sides.

[0095] Table 4 Appearance qualification rate of magnetic beads produced in batches under different preparation conditions

[0096] Preparation conditions Example 1 Example 2 Comparative Example 3 Appearance qualification rate (%) 69.80% 90.50% 54.60%

[0097] As can be seen from Table 4, Examples 1 and 2 adopt the ferrite beads preparation method provided by the present invention and use the optimized three-stage sintering process curve. The product appearance qualification rate obtained in the batch production position is significantly higher than that of the beads prepared by the conventional sintering method in Example 3.

[0098] At the same time, after cutting the green body, Example 2 uses a specific debinding curve for debinding, which is more conducive to significantly improving the appearance qualification rate of the product compared to Example 1 without debinding treatment; the appearance qualification rate of the magnetic beads prepared by the method of Example 2 can be as high as 90.5%. It can be seen that the combination of the optimized sintering temperature process and the debinding process provided by the present invention can greatly improve the appearance qualification rate of products in mass production and improve production efficiency.

[0099] In summary, the magnetic bead products prepared by the preparation method of ferrite magnetic beads provided by the present invention have high impedance in the specific frequency band of 100-400MHz, and have low DC resistance and large current characteristics compared to the magnetic beads prepared by conventional printing and sintering methods. At the same time, the products manufactured by the method of the present invention have a high appearance qualification rate and have high feasibility for mass production.

[0100] The product's unique air gap manufacturing method enables it to have excellent bias characteristics, and it can still maintain high performance, high reliability, and high stability in high-power load application scenarios. It can be widely used in audio noise reduction circuits, adapters, new energy vehicles and other fields, and has extremely high application value.

[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing ferrite beads, characterized in that: The following steps are involved: (1) printing an air gap layer on a ferrite base layer; the ferrite base layer is a perforated ferrite diaphragm, and the magnetic permeability of the material of the air gap layer is 0.01-10H / m; (2) printing a silver inner electrode and a filling material on the air gap layer to obtain a dielectric layer membrane; the thickness of the silver inner electrode is ≥80 μm; (3) stacking and cutting the dielectric diaphragm, and then sintering in three stages to obtain a semi-finished magnetic bead; in the three stages of sintering, the temperature of the first stage is 210-230° C., the temperature of the second stage is 260-280° C., and the temperature of the third stage is 890-910° C.; (4) Making external electrodes on the semi-finished magnetic beads to obtain the ferrite magnetic beads.

2. The method for preparing ferrite beads according to claim 1, characterized in that: In the step (1), the material of the air gap layer is NiZn ferrite.

3. The method for preparing ferrite beads according to claim 1, characterized in that: In the steps (1) and (2), the ferrite base layer and the filling material contain main ferrite magnetic powder, and the magnetic permeability of the main ferrite magnetic powder is 50-60H / m.

4. The method for preparing ferrite beads according to claim 3, characterized in that: In the step (2), the filling material is prepared by mixing and rolling the main ferrite magnetic powder, the carrier and the solvent to obtain a printing paste, which is the filling material.

5. The method for preparing ferrite beads according to claim 1, characterized in that: In the step (2), the printing of the silver inner electrode is as follows: printing the silver inner electrode pattern, drying, and then repeatedly printing and drying on the silver inner electrode pattern until the thickness of the silver inner electrode is reached.

6. The method for preparing ferrite beads according to claim 5, characterized in that: In the step (2), the filling material is printed in the area outside the silver inner electrode to fill the height difference around the silver inner electrode.

7. The method for preparing ferrite beads according to claim 1, characterized in that: In the step (3), the average heating rate of the first sintering stage is 0.8-1.2°C / min; the average heating rate of the second sintering stage is 0.05-0.12°C / min; and the average heating rate of the third sintering stage is 0.1-1.5°C / min.

8. The method for preparing ferrite beads according to claim 7, characterized in that: In the step (3), the first stage of sintering is: heating from 40°C to 220°C at an average heating rate of 1°C / min, and then keeping the temperature for 3.5-4.5h; The second stage of sintering is: heating from 220°C to 250°C at an average heating rate of 0.1-0.12°C / min, and then heating from 250°C to 270°C at an average heating rate of 0.06-0.07°C / min, and then keeping the temperature for 4.5-5.5h; The third stage of sintering is: heating from 270°C to 300°C at an average heating rate of 0.1°C / min, then heating from 300°C to 450°C at an average heating rate of 0.5°C / min, and then heating from 450°C to 900°C at an average heating rate of 1.5°C / min, and keeping warm for 3.5-4.5h.

9. The method for preparing ferrite beads according to claim 1, characterized in that: In the step (3), the dielectric diaphragms are stacked and cut to obtain green compacts, and after the green compacts are debinded, three-stage sintering is performed.

10. The ferrite beads prepared by the method for preparing ferrite beads according to any one of claims 1 to 9.