Modified cobaltosic oxide as well as preparation method and application thereof

Co-precipitation of cobalt-aluminum mixed solution and oxidant in parallel, and the reaction process is adjusted by complexing agent, and a high density and good particle size distribution of cobalt tetroxide was prepared, which solved the problem of unstable performance of cobalt tetroxide in the existing technology, significantly improving the The electrochemical properties and mechanical strength of the material are obtained.

CN118929776APending Publication Date: 2024-11-12TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310516117.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when preparing small-particle cobalt tetroxide, it is difficult to control the particle size and density, resulting in unstable product performance, and it is easy to produce fine powder during the synthesis process, affecting the particle size distribution and mechanical strength.

Method used

Cobalt-aluminum mixed solution and oxidant co-precipitate together. The oxidation degree and growth process of the initial reaction are adjusted by complexing agent, the density and particle size of the precipitate are controlled, and the growth of spherical cobalt oxide precipitates is achieved, and the material is retained by high-temperature calcination. Porous properties.

Benefits of technology

A high mechanical strength and density of cobalt oxide material was achieved, which significantly improved the electrochemical performance, and adjusted the particle shape by adjusting the proportion of complexing agent, and obtained good particle size distribution and tap density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929776A_ABST
    Figure CN118929776A_ABST
Patent Text Reader

Abstract

The invention provides modified cobaltosic oxide and a preparation method and application thereof, and the preparation method comprises the following steps: (1) adding a cobalt-aluminum mixed solution and an oxidizing agent into a base solution in a parallel flow manner, and carrying out a co-precipitation reaction to obtain a primary particle crystal nucleus; (2) standing and settling the primary particle crystal nucleus, removing 1 / 3-2 / 3 of supernate, adding a cobalt-aluminum mixed solution, an oxidizing agent, a mixed solution A and a mixed solution B in a parallel flow manner, carrying out growth reaction, concentrating, adjusting the pH value, and aging, so as to obtain a cobalt-aluminum mixed precipitate; and (3) carrying out calcination treatment on the cobalt-aluminum mixed precipitate to obtain the modified cobaltosic oxide, wherein the mixed solution A comprises a complexing agent A and sodium hydroxide, and the mixed solution B comprises a complexing agent B and cobalt metal salt. According to the method, the high mechanical strength and density of the material are guaranteed, the porous property of the material is reserved as much as possible, and the lithium cobalt oxide material prepared from the material shows excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and relates to modified cobalt tetroxide and a preparation method and application thereof. Background Art

[0002] Cobalt tetroxide is the main raw material for lithium cobalt oxide positive electrode. With the rapid development of smart devices, the performance requirements of lithium cobalt oxide positive electrode materials are getting higher and higher, and the product indicators of cobalt tetroxide are more stringent. The preparation method of cobalt tetroxide mainly adopts carbonate system and hydroxide system.

[0003] At present, the preparation of large-particle cobalt tetroxide by various manufacturers adopts carbonate system. The carbonate system precipitates cobalt through carbonates such as ammonium bicarbonate and ammonium carbonate. The conditions are relatively mild and the particles are easy to grow. It has a good advantage in preparing large-particle cobalt tetroxide. However, it is difficult to obtain initial crystal nuclei with smaller particle size when using carbonate system to prepare small-particle cobalt tetroxide, resulting in smaller reaction particle size growth space, shorter total reaction time and lower production capacity. At the same time, the crystallinity of cobalt carbonate is poor. The subsequent calcination of cobalt carbonate and the process of mixing cobalt with lithium will cause the cobalt tetroxide particles to be pulverized and broken due to low particle density. At the same time, the sedimentation rate of small-particle cobalt carbonate in the synthesis process is slow, and it is difficult to concentrate. If the carbonate system obtains crystal nuclei with smaller initial particle size by increasing the stirring intensity of the equipment, it will lead to the dissolution of cobalt under high stirring intensity, resulting in an increase in the cobalt content of the mother liquor, which is not conducive to the complete precipitation of cobalt.

[0004] CN101279771A discloses a method for preparing doped cobalt tetroxide, comprising: 1) mixing a cobalt nitrate solution containing doping element ions with a mixed precipitant solution containing ammonia water and sodium hydroxide, and reacting for 8 to 20 hours at a pH value of 8.4 to 10 and a temperature of 40 to 80° C. to obtain a cobalt hydroxide precipitate containing the doping element; 2) washing and drying the obtained cobalt hydroxide precipitate containing the doping element, and then calcining at a temperature of 500 to 800° C. for 2 to 6 hours to obtain doped cobalt tetroxide.

[0005] CN108373175A discloses a method for preparing aluminum-doped cobalt oxide, comprising the following steps: (1) mixing an aluminum salt solution with a complexing agent to obtain a mixed solution; (2) adding a cobalt salt solution, a precipitant solution containing carbonate ions, and the mixed solution obtained in step (1) to a reaction device in a parallel flow manner to coprecipitate to obtain aluminum-doped cobalt carbonate; and (3) calcining the aluminum-doped cobalt carbonate obtained in step (2) to obtain aluminum-doped cobalt oxide.

[0006] The doped cobalt tetroxide product prepared by the above scheme is prone to produce fine powder during the synthesis process due to the uneven precipitation of Al, and the product particle size distribution is too wide, which affects the product performance. Summary of the invention

[0007] The purpose of the present invention is to provide a modified cobalt oxide and a preparation method and application thereof. The method of the present invention ensures high mechanical strength and density of the material while retaining the porous properties of the material as much as possible. The lithium cobalt oxide material prepared by the method shows excellent electrochemical properties.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing modified cobalt trioxide, the preparation method comprising the following steps:

[0010] (1) adding the cobalt-aluminum mixed solution and the oxidant into the bottom liquid in parallel to perform a coprecipitation reaction to obtain primary particle crystal nuclei;

[0011] (2) After the primary particle nuclei are allowed to settle, 1 / 3 to 2 / 3 of the supernatant is removed, and a cobalt-aluminum mixed solution, an oxidant, a mixed solution A and a mixed solution B are added to carry out a growth reaction, and after concentration, the pH is adjusted and aged to obtain a cobalt-aluminum mixed precipitate;

[0012] (3) calcining the cobalt-aluminum mixed precipitate to obtain the modified cobalt tetroxide;

[0013] Wherein, the mixed solution A includes complexing agent A and sodium hydroxide, and the mixed solution B includes complexing agent B and cobalt metal salt.

[0014] The invention controls the oxidation degree of the materials in the initial stage of the reaction by adjusting the complexing agent and the adding method of the complexing agent, oxidizes the precipitate into spherical cobalt oxide precipitate crystal nuclei with high density and small particle size, and then grows by adjusting the complexing agent to prepare a spherical cobalt-aluminum mixed precipitate with no pores and high density.

[0015] In the reaction growth stage, the present invention uses the regulating effect of the mixed solution B containing the complexing agent B to make the primary cobalt tetraoxide particles that are not conducive to growth be wrapped and grown by cobalt oxyhydroxide or cobalt hydroxide, so as to achieve the growth of particles. At the same time, under the action of the complexing agent A in the mixed solution A, the precipitate is more likely to achieve dense growth, and avoids growing too fast under the action of the complexing agent B. At the same time, by adjusting the ratio of the complexing agent A to the complexing agent B, the shape of the primary particles can be adjusted, so that the cobalt-aluminum mixed precipitate grows densely.

[0016] Preferably, the complexing agent A includes any one of ammonia water, ammonium sulfate, ammonium bicarbonate or ammonium carbonate, or a combination of at least two thereof.

[0017] Preferably, the complexing agent B includes any one of EDTA, tartaric acid or hydroxycarboxylic acid or a combination of at least two thereof.

[0018] Preferably, the base liquid in step (1) comprises pure water, complexing agent A and an oxidant.

[0019] Preferably, the oxidant comprises hydrogen peroxide.

[0020] Preferably, the pH of the base solution is 11-12.5, for example, 11, 11.2, 11.5, 12 or 12.5.

[0021] Preferably, the hourly flow rate of the cobalt-aluminum mixed solution in step (1) is 1 / 30 to 1 / 10 of the volume of the reaction container, for example: 1 / 30, 1 / 25, 1 / 20, 1 / 15 or 1 / 10.

[0022] Preferably, the molar ratio of the oxidant to cobalt is (0.4-0.8):1, for example: 0.4:1, 0.5:1, 0.6:1, 0.7:1 or 0.8:1, etc.

[0023] Preferably, the temperature of the coprecipitation reaction in step (1) is 55-85°C, for example, 55°C, 60°C, 65°C, 70°C or 85°C.

[0024] Preferably, the pH of the coprecipitation reaction is 11-12.5, for example, 11, 11.2, 11.5, 12 or 12.5.

[0025] Preferably, the coprecipitation reaction time is 4 to 12 hours, for example: 4 hours, 6 hours, 8 hours, 10 hours or 12 hours.

[0026] Preferably, the median particle size D50 of the primary particle nuclei is 0.5-1.5 μm, for example, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm or 1.5 μm.

[0027] Preferably, the concentration of sodium hydroxide in the mixed solution A in step (2) is 200-400 g / L, for example, 200 g / L, 250 g / L, 300 g / L, 350 g / L or 400 g / L.

[0028] Preferably, the concentration of the complexing agent A in the mixed solution A is 0.1-20 g / L, for example, 0.1 g / L, 10 g / L, 2 g / L, 5 g / L, 10 g / L or 20 g / L.

[0029] Preferably, the concentration of the cobalt salt in the mixed solution B is 80-140 g / L, for example, 80 g / L, 90 g / L, 100 g / L, 120 g / L or 140 g / L.

[0030] Preferably, the concentration of the complexing agent B in the mixed solution B is 0.1-2 g / L, for example, 0.1 g / L, 0.5 g / L, 1 g / L, 1.5 g / L or 2 g / L.

[0031] Preferably, the molar ratio of cobalt to aluminum in the mixed solution B is 100:(0.1-4.8), for example: 100:0.1, 100:0.5, 100:1, 100:2 or 100:4.8, etc.

[0032] Preferably, the pH of the growth reaction in step (2) is 9.5-12, for example: 9.5, 10, 10.5, 11 or 12, etc.

[0033] Preferably, the growth reaction temperature is 55-85°C, for example, 55°C, 60°C, 65°C, 70°C or 85°C.

[0034] Preferably, the method of adjusting the pH comprises adding sodium hydroxide.

[0035] Preferably, the pH is 11-12, for example, 11, 11.2, 11.5, 11.8 or 12.

[0036] Preferably, the aging time is 1 to 2 hours, for example: 1 hour, 1.2 hours, 1.5 hours, 1.8 hours or 2 hours.

[0037] Preferably, the cobalt compound in the cobalt-aluminum mixed precipitate in step (2) includes any one of cobalt oxyhydroxide, cobalt hydroxide or cobalt trioxide, or a combination of at least two of them.

[0038] Preferably, the mass fraction of the cobalt element in the cobalt-aluminum mixed precipitate is 60-65%, for example, 60%, 61%, 62%, 63%, 64% or 65%.

[0039] Preferably, the tap density of the cobalt-aluminum mixed precipitate is >2.3 g / cm 3 .

[0040] Preferably, the cobalt-aluminum mixed precipitate has a dense sphere with block-shaped and / or strip-shaped primary particles interwoven.

[0041] Preferably, the temperature of the calcination treatment in step (3) is 700-850°C, for example, 700°C, 720°C, 750°C, 800°C or 850°C.

[0042] Preferably, the calcination treatment time is 2 to 8 hours, for example: 2 hours, 3 hours, 5 hours, 6 hours or 8 hours.

[0043] Preferably, the calcination treatment is followed by a water washing and impurity removal treatment.

[0044] In a second aspect, the present invention provides a modified cobalt oxide, wherein the modified cobalt oxide is prepared by the method described in the first aspect.

[0045] Preferably, the mass fraction of the cobalt element in the modified cobalt tetroxide is 71-73%, for example, 71%, 71.5%, 72%, 72.5% or 73%.

[0046] Preferably, the morphology of the modified cobalt oxide includes porous secondary spherical particles composed of spherical or quasi-spherical primary particles.

[0047] Preferably, the diameter of the primary ion is 100-500 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm or 500 nm.

[0048] Preferably, the aluminum content of the modified cobalt oxide is 2000-16000 ppm, for example, 2000 ppm, 4000 ppm, 5000 ppm, 8000 ppm, 10000 ppm or 16000 ppm.

[0049] Preferably, the laser particle size of the modified cobalt oxide is D50=2-6 μm, (D90-D10) / D50=0.4-0.9.

[0050] Preferably, the tap density of the modified cobalt oxide is >2.2 g / cm 3 .

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] (1) The present invention adds an oxidant before the reaction is started, and oxidizes it into primary cobalt oxide particles with higher density and smaller particle size with the assistance of complexing agent A, which can effectively increase the number of nuclei, extend the total reaction cycle by more than 60 hours, and improve production efficiency. At the same time, the prepared precipitate has no pores inside and high density, which is conducive to the sedimentation and concentration of materials during the synthesis process, and reduces the requirements for concentration equipment. On the other hand, the high particle density and slow particle growth rate during the reaction process are conducive to the uniform precipitation of aluminum.

[0053] (2) In the reaction growth stage, the cobalt oxide primary particles that are not conducive to growth are wrapped and grown by cobalt oxyhydroxide or cobalt hydroxide through the regulating effect of the complexing agent B, so that the particles grow. At the same time, under the action of the complexing agent A, the precipitate is more likely to achieve dense growth, avoiding excessive growth under the action of the complexing agent B. At the same time, by adjusting the ratio of the complexing agent A to the complexing agent B, the shape of the primary particles can be adjusted, so that the cobalt-aluminum mixed precipitate grows densely.

[0054] (3) After high-temperature calcination, the cobalt-aluminum mixed precipitate of the present invention, on the one hand, will leave a large number of pores when the water decomposed inside the particles is discharged, which is convenient for the elution of internal impurities during the secondary water washing, and is also conducive to the infiltration of lithium during the later sintering process of the positive electrode material. On the other hand, water molecules are flexible molecules, and the process of escaping will not damage the inside of the particles, retaining the high density while inheriting the high mechanical strength of the hydroxide particles.

[0055] (4) The (D90-D10) / D50 of the modified cobalt tetraoxide prepared by the method of the present invention can reach below 0.45, showing a good particle size distribution and a tap density of up to 2.41 g / cm 3 above. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a 1000x SEM image of the cobalt-aluminum mixed precipitate described in Example 1.

[0057] Figure 2 This is a 10,000-fold SEM image of the cobalt-aluminum mixed precipitate described in Example 1.

[0058] Figure 3 This is a 5000-fold SEM image of the modified cobalt oxide described in Example 1.

[0059] Figure 4 This is a 30,000-fold SEM image of the modified cobalt tetroxide described in Example 1.

[0060] Figure 5 This is a 1000x SEM image of the cobalt-aluminum mixed precipitate described in Example 3.

[0061] Figure 6 This is a 10,000-fold SEM image of the cobalt-aluminum mixed precipitate described in Example 3.

[0062] Figure 7 This is a 5000-fold SEM image of the modified cobaltous oxide described in Example 3.

[0063] Figure 8 This is a 30,000-fold SEM image of the modified cobalt oxide described in Example 3.

[0064] Fig. 9 This is a 3000-fold SEM image of the cobalt-aluminum mixed precipitate described in Example 4.

[0065] Fig.10 This is a 3000-fold SEM image of the modified cobaltous oxide described in Example 4.

[0066] Fig.11 This is a 5000x SEM image of the cross section of the modified cobalt oxide described in Example 1.

[0067] Fig.12 3000 times SEM image of the modified cobalt tetroxide described in Comparative Example 1.

[0068] Fig.13 SEM image of the modified cobaltous oxide and lithium carbonate mixed as described in Example 1. DETAILED DESCRIPTION

[0069] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0070] Example 1

[0071] This embodiment provides a modified cobalt oxide, and the preparation method of the modified cobalt oxide is as follows:

[0072] (1) Prepare a mixed solution A with a sodium hydroxide concentration of 400 g / L and an ammonia concentration of 5 g / L; prepare a mixed solution B with a cobalt concentration of 100 g / L, an aluminum ion concentration of 0.68 g / L, and an EDTA concentration of 1.2 g / L; prepare a 15% hydrogen peroxide solution, add 2 L of pure water to a 5 L reactor, start stirring at 1000 rpm, heat the bottom solution to 75 ± 2 ° C, add ammonia water and sodium hydroxide solution, adjust the bottom solution pH to 11.2-11.4, and adjust the ammonia concentration to 15 g / L , pre-introduce compressed air into the bottom liquid of the reactor for 2 hours, the compressed air flow rate is 0.5L / min, and start the reaction after adding 20ml of 15% hydrogen peroxide. The flow rate of cobalt-aluminum mixed salt solution (the only difference from mixed solution B is that EDTA is not added) is 3ml / min, the flow rate of hydrogen peroxide is 0.9ml / min, the stirring speed is 1000rpm, and the flow rate of alkali solution is adjusted to maintain the pH value of 11.2-11.4 for 5 hours to obtain the primary particle nucleus with a laser particle size of about 1μm;

[0073] (2) Transfer the primary particle nuclei to the growth reactor, drain 1 / 2 volume of the supernatant by sedimentation, and add cobalt-aluminum mixed solution, hydrogen peroxide solution, mixed solution A and mixed solution B, maintain the reaction temperature at 75°C and pH 9.3-9.5 for growth. After the reactor is full, use a concentration device to concentrate the overflow material, discharge the mother liquor and return the remaining material to the reactor to continue the reaction. During the reaction, the particle size is tested every hour. When the particle size is 3 μm, the feed is stopped, the pH is adjusted to 11.8-12 for aging for 1 hour, and after the aging is completed, the final slurry is washed and dried to obtain a cobalt-aluminum mixed precipitate. The SEM image of the cobalt-aluminum mixed precipitate is shown in the figure. Figure 1-2 As shown;

[0074] (3) pre-calcining the dried material at 300° C. for 2 h, sintering at 760° C. for 4 h, washing twice to remove impurities, and finally obtaining the modified cobalt tetroxide after post-treatment;

[0075] The SEM image of the modified cobalt tetroxide is as follows: Figure 3-4 As shown by Figure 3-4 It can be seen that the particle size distribution of the modified cobalt oxide prepared by the present invention is uniform. Fig.11 ,Depend on Fig.11 It can be seen that the pore size distribution inside the modified cobalt tetroxide prepared by the present invention is uniform. The microscopic morphology of the cobalt tetroxide mixed with lithium carbonate is shown in the electron microscope image. Fig.13 shown.

[0076] Example 2

[0077] This embodiment provides a modified cobalt oxide, and the preparation method of the modified cobalt oxide is as follows:

[0078] (1) Prepare a mixed solution A with a sodium hydroxide concentration of 400 g / L and an ammonia concentration of 5 g / L; prepare a mixed solution B with a cobalt concentration of 100 g / L, an aluminum ion concentration of 0.68 g / L, and an EDTA concentration of 1.2 g / L; prepare a 15% hydrogen peroxide solution, add 2 L of pure water to a 5 L reactor, start stirring at 1000 rpm, heat the bottom solution to 73 ± 2 °C, add ammonia and sodium hydroxide solution, and adjust the bottom solution pH to 11. -11.2, ammonia concentration 15g / L, pre-introduce compressed air into the bottom liquid of the reactor for 2H, the compressed air flow rate is 0.5L / min, add 20ml of 15% hydrogen peroxide to start the reaction, the flow rate of cobalt-aluminum mixed salt solution (the only difference from mixed solution B is that EDTA is not added) is 3ml / min, the flow rate of hydrogen peroxide is 0.9ml / min, the stirring speed is 1000rpm, and the alkali solution flow rate is adjusted to maintain the pH value of 11-11.2 for 5h to obtain the primary particle nucleus with a laser particle size of about 1μm;

[0079] (2) Transfer the primary particle nucleus to the growth kettle, drain 1 / 2 volume of supernatant by sedimentation, add cobalt-aluminum mixed solution, hydrogen peroxide solution, mixed solution A and mixed solution B, maintain the reaction temperature at 75°C and pH 10.8-11 for growth, use the concentration device to concentrate the overflow material after the reactor is full, discharge the mother liquor and return the remaining material to the reactor to continue the reaction. During the reaction, the particle size is tested every hour, and the feeding is stopped when the particle size is 3 μm. The pH is adjusted to 11.5-11.8 for aging for 1 hour. After the aging is completed, the final slurry is washed and dried to obtain a cobalt-aluminum mixed precipitate;

[0080] (3) The dried material is pre-calcined at 320° C. for 2 h, and then sintered at 750° C. for 4 h. The material is washed twice to remove impurities, and then post-treated to finally obtain the modified cobalt tetroxide.

[0081] Example 3

[0082] The only difference between this embodiment and embodiment 1 is that the aluminum content in the mixed solution B and the cobalt-aluminum mixed salt solution is 1.68 g / L, and the other conditions and parameters are exactly the same as those in embodiment 1. Figure 5-6 As shown, the SEM image of modified cobalt tetroxide is as follows Figure 7-8 shown.

[0083] Example 4

[0084] The difference between this embodiment and embodiment 1 is that, instead of adding hydrogen peroxide in step (2), compressed air is introduced at a flow rate of 1.5 L / min. The other conditions and parameters are exactly the same as those in embodiment 1. Fig. 9 As shown, the SEM image of modified cobalt tetroxide is as follows Fig.10 shown.

[0085] Comparative Example 1

[0086] The only difference between this comparative example and Example 1 is that EDTA is not added to the mixed solution B during the growth stage, and the other conditions and parameters are exactly the same as those of Example 1. The SEM image of the obtained cobalt trioxide is as follows: Fig.12 shown.

[0087] Performance Test:

[0088] The properties of the modified cobalt trioxide obtained in the test examples and comparative examples are shown in Table 1:

[0089] Table 1

[0090] D50(μm) (D90-D10) / D50 Aluminum content (ppm) <![CDATA[Tap density (g / cm 3 )]]> Example 1 3.219 0.45 4278 2.41 Example 2 3.143 0.42 4412 2.45 Example 3 3.119 0.59 12025 2.54 Example 4 3.018 0.63 4285 2.24 Comparative Example 1 3.201 1.21 4276 2.01

[0091] As can be seen from Table 1, from Examples 1-2, the (D90-D10) / D50 of the modified cobalt tetraoxide prepared by the method of the present invention can reach less than 0.45, showing a good particle size distribution, and the tap density can reach 2.41 g / cm 3 above.

[0092] By comparing Example 1 and Example 3, it can be seen that Figure 1-2 and Figure 5-6 as well as Figure 3-4 and Figure 7-8By comparison, it can be seen that the cobalt-aluminum molar ratio (i.e., the content of cobalt and aluminum in the cobalt-aluminum mixed solution) will affect the morphology and properties of the modified cobalt tetroxide. When the cobalt-aluminum molar ratio is controlled at 100:0.1-4.8, the performance of the modified cobalt tetroxide is better. If the aluminum content is too high, although the tap density is improved, the uniformity of the particle size distribution of the obtained cobalt tetroxide is significantly reduced.

[0093] By comparing Example 1 and Example 4, it can be seen that Figure 1-2 and Fig. 9 as well as Figure 3-4 and Fig.10 By comparison, it can be seen that when the oxidant is replaced by compressed air, the particle size distribution and true density of the obtained material are significantly deteriorated, because the oxidation effect of compressed air is worse than that of the oxidant, and the oxidation degree of the material in the initial stage of the reaction cannot be well controlled.

[0094] By comparing Example 1 with Comparative Example 1, Figure 3-4 and Fig.12 By comparison, it can be seen that the present invention can adjust the shape of the primary particles by adjusting the addition method of the complexing agent, so that the cobalt-aluminum mixed precipitate can grow densely.

[0095] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing modified cobalt tetroxide, characterized in that: The preparation method comprises the following steps: (1) adding the cobalt-aluminum mixed solution and the oxidant into the bottom liquid in parallel to perform a coprecipitation reaction to obtain primary particle crystal nuclei; (2) After the primary particle nuclei are allowed to settle, 1 / 3 to 2 / 3 of the supernatant is removed, and a cobalt-aluminum mixed solution, an oxidant, a mixed solution A and a mixed solution B are added to carry out a growth reaction, and after concentration, the pH is adjusted and aged to obtain a cobalt-aluminum mixed precipitate; (3) calcining the cobalt-aluminum mixed precipitate to obtain the modified cobalt tetroxide; Wherein, the mixed solution A includes complexing agent A and sodium hydroxide, and the mixed solution B includes complexing agent B and cobalt metal salt.

2. The preparation method according to claim 1, characterized in that The complexing agent A includes any one of ammonia water, ammonium sulfate, ammonium bicarbonate or ammonium carbonate, or a combination of at least two thereof; Preferably, the complexing agent B includes any one of EDTA, tartaric acid or hydroxycarboxylic acid or a combination of at least two thereof.

3. The preparation method according to claim 1 or 2, characterized in that: The base solution in step (1) comprises pure water, complexing agent A and an oxidant; Preferably, the oxidant comprises hydrogen peroxide; Preferably, the pH of the base solution is 11-12.

5.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The hourly flow rate of the cobalt-aluminum mixed solution in step (1) is 1 / 30 to 1 / 10 of the volume of the reaction container; Preferably, the molar ratio of the oxidant to cobalt is (0.4-0.8):

1.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The temperature of the coprecipitation reaction in step (1) is 55-85° C. Preferably, the pH of the coprecipitation reaction is 11 to 12.5; Preferably, the coprecipitation reaction time is 4 to 12 hours; Preferably, the median particle size D50 of the primary particle nucleus is 0.5-1.5 μm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The concentration of sodium hydroxide in the mixed solution A of step (2) is 200-400 g / L; Preferably, the concentration of the complexing agent A in the mixed solution A is 0.1 to 20 g / L; Preferably, the concentration of the cobalt salt in the mixed solution B is 80-140 g / L; Preferably, the concentration of the complexing agent B in the mixed solution B is 0.1 to 2 g / L; Preferably, the molar ratio of cobalt to aluminum in the mixed solution B is 100:(0.1-4.8).

7. The preparation method according to any one of claims 1 to 6, characterized in that: The pH of the growth reaction in step (2) is 9.5 to 12; Preferably, the temperature of the growth reaction is 55-85°C; Preferably, the method of adjusting pH comprises adding sodium hydroxide; Preferably, the pH is 11 to 12; Preferably, the aging time is 1 to 2 hours.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The cobalt compound in the cobalt-aluminum mixed precipitate of step (2) includes any one of cobalt oxyhydroxide, cobalt hydroxide or cobalt trioxide, or a combination of at least two thereof; Preferably, the mass fraction of cobalt element in the cobalt-aluminum mixed precipitate is 60-65%; Preferably, the tap density of the cobalt-aluminum mixed precipitate is >2.3 g / cm 3 ; Preferably, the cobalt-aluminum mixed precipitate has a morphology of dense spheres interwoven with block-shaped and / or strip-shaped primary particles.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The calcination temperature in step (3) is 700-850°C; Preferably, the calcination treatment time is 2 to 8 hours; Preferably, the calcination treatment is followed by a water washing and impurity removal treatment.

10. A modified cobalt trioxide, characterized in that: The modified cobalt trioxide is prepared by the method according to any one of claims 1 to 9; Preferably, the mass fraction of cobalt element in the modified cobalt tetroxide is 71-73%; Preferably, the morphology of the modified cobalt oxide includes porous secondary spherical particles composed of spherical or quasi-spherical primary particles; Preferably, the diameter of the primary ion is 100 to 500 nm; Preferably, the aluminum content in the modified cobalt oxide is 2000 to 16000 ppm; Preferably, the laser particle size of the modified cobalt oxide is D50=2-6 μm, (D90-D10) / D50=0.4-0.9; Preferably, the tap density of the modified cobalt oxide is >2.2 g / cm 3 .

Citation Information

Cited By

  • Spherical cobaltosic oxide as well as preparation method and application thereof

    CN120622551A

  • Rare earth doped cobaltosic oxide, preparation method thereof and lithium cobalt oxide material

    CN121672592A