Preparation method of aluminum-doped cobaltous hydroxide
By using sodium sulfide as a reducing agent and complexing agent in the preparation of aluminum doped cobalt hydroxide, the high doping amount and uniform distribution of α-type aluminum doped cobalt hydroxide are achieved, and aluminum doping hydroxide in the prior art is solved The difficulty of cobalt sub-process and uneven distribution of aluminum reduce the preparation cost and are suitable for large-scale production.
Patent Information
- Application Number
- CN202411171934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing aluminum-doped cobalt hydroxide preparation process is difficult to achieve uniform distribution of elements. Especially under high aluminum doping, the preparation process of α-type aluminum-doped cobalt hydroxide is difficult and the aluminum distribution uniformity is poor.
Using sodium sulfide as a reducing agent, combined with the reaction of complexing agent and anaerobic conditions, high-purity alpha-type aluminum-doped cobalt hydroxide was prepared, which improved the doping amount and distribution uniformity of aluminum and reduced the difficulty of preparation process. and cost.
The high doping amount and uniform distribution of aluminum in α-type aluminum doped cobalt hydroxide is achieved, with small morphological differences and suitable for large-scale production. The aluminum doping amount is stable between 6000-10000ppm, and the aluminum doping amount varies by small difference between different sampling points.
Smart Images

Figure CN118929779A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrode materials, and in particular to a method for preparing aluminum-doped cobaltous hydroxide. Background Art
[0002] Aluminum-doped cobaltous hydroxide is often used to coat lithium cobalt oxide positive electrode materials, thereby reducing the direct contact between the positive electrode material surface and the electrolyte, thereby reducing cobalt dissolution and gas production, and improving its electrochemical properties such as storage and gas production.
[0003] At present, when cobaltous hydroxide is doped with aluminum, it is difficult to achieve co-precipitation and uniform distribution of elements due to the large difference in the precipitation rates of aluminum and cobalt. Aluminum-doped cobaltous hydroxide includes α-type aluminum-doped cobaltous hydroxide and β-type aluminum-doped cobaltous hydroxide. Among them, β-type aluminum-doped cobaltous hydroxide is a brucite-like structure with low activity, and α-type aluminum-doped cobaltous hydroxide is a hydrotalcite structure with a larger lattice spacing, which can expose more active sites and has a better sintering effect. It can promote the transfer rate of Li in the material and obtain better electrochemical properties. At the same time, a larger interlayer spacing is also conducive to the diffusion of aluminum, improving the uniformity of aluminum distribution when doping aluminum, and indirectly improving the dispersion of aluminum in cobaltous hydroxide.
[0004] However, since β-type aluminum-doped cobaltous hydroxide is a thermally stable phase, while α-type aluminum-doped cobaltous hydroxide is a metastable state, the preparation process of α-type aluminum-doped cobaltous hydroxide is difficult. As the amount of aluminum doping increases, the preparation process of α-type aluminum-doped cobaltous hydroxide becomes more difficult, accompanied by a decrease in the uniformity of aluminum element distribution. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned related technologies, the present application provides a method for preparing aluminum-doped cobaltous hydroxide. The present application adopts sodium sulfide as a reducing agent, cooperates with a complexing agent, and reacts under anaerobic conditions to prepare high-purity α-type aluminum-doped cobaltous hydroxide, thereby increasing the doping amount of aluminum in the α-type aluminum-doped cobaltous hydroxide, and in the case of a high doping amount of aluminum in the α-type aluminum-doped cobaltous hydroxide, the uniformity of the distribution is improved, and the morphological difference is reduced.
[0006] The present application provides a method for preparing aluminum-doped cobaltous hydroxide using the following technical solution: A preparation method of aluminum-doped cobaltous hydroxide comprises the following steps: mixing a cobalt-aluminum mixed solution, an alkaline solution, a complexing agent, sodium sulfide and deionized water to obtain a mixed solution, stirring and reacting the mixed solution at a constant temperature of 40-90°C under an anaerobic condition for 1-2 hours, and then drying the mixed solution to obtain a precursor material, and grinding and sieving the precursor material to obtain aluminum-doped cobaltous hydroxide.
[0007] Preferably, the molar ratio of the sodium sulfide to the cobalt ions in the cobalt-aluminum mixed solution is 0.003-0.004:1.
[0008] Preferably, the molar ratio of the sodium sulfide to the cobalt ions in the cobalt-aluminum mixed solution is 0.0032:1.
[0009] Preferably, the cobalt ion concentration in the cobalt-aluminum mixed solution is 1-2.5 mol / L, and the aluminum ion concentration is 0.02-0.06 mol / L.
[0010] Preferably, the cobalt ion concentration in the cobalt-aluminum mixed solution is 2 mol / L, and the aluminum ion concentration is 0.051 mol / L.
[0011] Preferably, in the aluminum-cobalt mixed solution, the molar ratio of cobalt ions to aluminum ions is 1:0.02-0.04.
[0012] Preferably, in the aluminum-cobalt mixed solution, the molar ratio of cobalt ions to aluminum ions is 1:0.0255.
[0013] Preferably, the cobalt salt in the cobalt-aluminum mixed aqueous solution is one or more of cobalt sulfate, cobalt chloride, and cobalt nitrate, and the aluminum salt is one or both of aluminum chloride and aluminum nitrate.
[0014] Preferably, the cobalt salt in the cobalt-aluminum mixed aqueous solution is cobalt sulfate, and the aluminum salt is aluminum chloride.
[0015] Preferably, the complexing agent comprises one or more of citric acid, ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate.
[0016] Preferably, the alkaline solution is one or both of a sodium hydroxide solution and a potassium hydroxide solution.
[0017] Preferably, the alkaline solution is a sodium hydroxide solution.
[0018] Preferably, the pH of the mixed solution is 8.5-10.5.
[0019] Preferably, the pH of the mixed solution is 9.5.
[0020] Preferably, the temperature during the constant temperature stirring reaction is 60°C.
[0021] Preferably, the drying is vacuum drying at a temperature of 80-100°C.
[0022] Preferably, the drying is vacuum drying at a drying temperature of 90°C.
[0023] Preferably, the screening condition is 200-500 mesh screening.
[0024] Preferably, the screening condition is 400 mesh screening.
[0025] Preferably, the aluminum-doped cobaltous hydroxide has an aluminum doping amount of 6000-10000 ppm.
[0026] Preferably, the aluminum-doped cobaltous hydroxide has an aluminum-doped content of 6551-8357 ppm.
[0027] In summary, the present application includes at least one of the following beneficial technical effects: 1. The present application uses sodium sulfide as a reducing agent, a complexing agent and an oxygen-free reaction condition to prepare a high-purity α-type aluminum-doped cobalt hydroxide, thereby increasing the doping amount of aluminum in the α-type aluminum-doped cobalt hydroxide, and in the case of a high doping amount of aluminum in the α-type aluminum-doped cobalt hydroxide, the uniformity of the distribution is improved and the morphology difference is reduced; 2. The aluminum doping amount of the prepared α-type aluminum-doped cobaltous hydroxide is stable between 6000ppm and 10000ppm, and the difference in aluminum doping amount at different sampling points is within 5%.
[0028] 3. The preparation process of the α-type aluminum-doped cobaltous hydroxide of the present application is low in difficulty and mild in conditions, which reduces the preparation cost and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the X-ray diffraction pattern of aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1 in this application.
[0030] Figure 2 This is a scanning electron microscope image of aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1 in this application.
[0031] Figure 3 This is a scanning electron microscope image of aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 2 in this application.
[0032] Figure 4 This is a scanning electron microscope image of aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 3 in this application.
[0033] Figure 5 3 is a scanning electron microscope image of aluminum-doped cobaltous hydroxide prepared by the preparation method of Comparative Example 1. DETAILED DESCRIPTION
[0034] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.
[0035] The raw materials used in the examples and comparative examples can all be obtained commercially.
[0036] Example 1 Embodiment 1 of the present application provides a method for preparing aluminum-doped cobaltous hydroxide, and the specific steps are as follows: cobalt sulfate and aluminum chloride are used to prepare a cobalt-aluminum mixed solution with a cobalt ion concentration of 2 mol / L and an aluminum ion concentration of 0.051 mol / L, and disodium ethylenediaminetetraacetic acid and sodium sulfide are added to the cobalt-aluminum mixed solution to obtain a mixed solution, wherein the concentration of disodium ethylenediaminetetraacetic acid in the mixed solution is 1 g / L, and the concentration of sodium sulfide is 0.5 g / L; the mixed solution is mixed with a sodium hydroxide solution, and the pH is adjusted to 9.5 and then added to a reactor, and nitrogen is continuously introduced into the liquid at a flow rate of 7 kg / h, and stirred and mixed at 220 rpm. Then the temperature is raised to 60°C, the reaction is carried out at a constant temperature for 1.5 hours, and then the precursor material is dried in a vacuum at a temperature of 90°C to obtain the precursor material; the precursor material is ground and sieved at 400 mesh to obtain aluminum-doped cobaltous hydroxide.
[0037] Example 2 Example 2 of the present application provides a method for preparing aluminum-doped cobaltous hydroxide. The difference between Example 2 and Example 1 is that the cobalt ion concentration in the cobalt-aluminum mixed solution in Example 2 is 1 mol / L, and the aluminum ion concentration is 0.02 mol / L.
[0038] Example 3 Example 3 of the present application provides a method for preparing aluminum-doped cobaltous hydroxide. The difference between Example 3 and Example 1 is that in Example 3, citric acid is used to replace disodium ethylenediaminetetraacetic acid to prepare aluminum-doped cobaltous hydroxide.
[0039] Comparative Example 1 Comparative Example 1 provides a method for preparing aluminum-doped cobaltous hydroxide, and the specific steps are as follows: cobalt sulfate and aluminum chloride are used to prepare a cobalt-aluminum mixed solution with a cobalt ion concentration of 2 mol / L and an aluminum ion concentration of 0.051 mol / L, and ammonia water is added to the cobalt-aluminum mixed solution to obtain a mixed solution, wherein the concentration of ammonia in the mixed solution is 5 g / L; the mixed solution is mixed with a sodium hydroxide solution, and the pH is adjusted to 9.5 and then added to a reactor, and nitrogen is continuously introduced into the liquid at a flow rate of 7 kg / h, and stirred and mixed at 220 rpm. Then, the temperature is raised to 60°C, the reaction is carried out at a constant temperature for 1.5 hours, and then the precursor material is dried in a vacuum at a temperature of 90°C to obtain the precursor material; the precursor material is ground and sieved with 400 mesh to obtain aluminum-doped cobaltous hydroxide.
[0040] Test and Inspection (1) The aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1 was subjected to X-ray diffraction detection, and the X-ray diffraction pattern was as follows: Figure 1 shown.
[0041] (2) The aluminum-doped cobaltous hydroxide prepared by the preparation method of Examples 1 to 3 and Comparative Example 1 was detected by atomic emission spectrometry (ICP). The average aluminum-doped amount (ppm) was obtained by taking the average value of the aluminum-doped cobaltous hydroxide at different sampling points, as shown in Table 1 below.
[0042] Table 1:
[0043] (3) Scanning electron microscope imaging was performed on the aluminum-doped cobaltous hydroxide prepared by the preparation methods of Examples 1-3 and Comparative Example 1. Figure 2-5 shown.
[0044] Results Analysis The following combines Table 1 and Figure 1-5 The experimental results provided are used to explain this application in detail.
[0045] Reference Figure 1 It can be seen that the aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1 is a hexagonal α-type aluminum-doped cobaltous hydroxide. Figure 2 The aluminum-doped cobaltous hydroxide particles prepared by the preparation method of Example 1 are spherical and have little morphology difference.
[0046] Reference Figure 2-Figure 4 The aluminum-doped cobalt hydroxides prepared by the preparation methods of Examples 1-3 are all spherical and have small morphological differences. Figure 5 When ammonia water is used as a complexing agent and reducing agent, the scanning electron microscope image of the aluminum-doped cobaltous hydroxide obtained shows that small particles agglomerate to form irregular shapes with large morphological differences. Analysis shows that this is due to the insufficient complexing ability of ammonia water.
[0047] Referring to Table 1, the average aluminum doping amount of the aluminum-doped cobaltous hydroxide prepared by the preparation methods of Examples 1-3 all reached more than 6000 ppm, indicating that the aluminum-doped cobaltous hydroxide prepared by the preparation methods of Examples 1-3 was uniformly distributed and had small morphological differences under the condition of high aluminum doping amount; in particular, the aluminum doping amount of the aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1 was as high as 8357 ppm, indicating that when the cobalt ion concentration was 2 mol / L and the aluminum ion concentration was 0.051 mol / L, using disodium ethylenediaminetetraacetic acid as a complexing agent and using sodium sulfide as a reducing agent were beneficial to increasing the aluminum doping amount of the obtained aluminum-doped cobaltous hydroxide. Compared with the aluminum-doped cobaltous hydroxide prepared by the preparation method of Example 1, the aluminum-doped cobaltous hydroxide prepared by the preparation method of Comparative Example 1 uses ammonia water as a complexing agent and a reducing agent when the cobalt ion concentration and the aluminum ion concentration remain unchanged, resulting in a significant decrease in the aluminum content of the prepared aluminum-doped cobaltous hydroxide. Analysis shows that this is because the complexing ability of ammonia water alone as a complexing agent and a reducing agent for aluminum ions is weaker than the complexing ability of disodium ethylenediaminetetraacetate as a complexing agent and sodium sulfide as a reducing agent for aluminum ions.
[0048] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing aluminum-doped cobaltous hydroxide, characterized in that: The method comprises the following steps: mixing a cobalt-aluminum mixed solution, an alkaline solution, a complexing agent, sodium sulfide and deionized water to obtain a mixed solution, stirring the mixed solution at a constant temperature of 40-90°C under an anaerobic condition for 1-2 hours, and then drying the mixed solution to obtain a precursor material, and grinding and sieving the precursor material to obtain aluminum-doped cobaltous hydroxide.
2. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The molar ratio of the sodium sulfide to the cobalt ions in the cobalt-aluminum mixed solution is 0.003-0.004:
1.
3. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The cobalt ion concentration in the cobalt-aluminum mixed solution is 1-2.5 mol / L, and the aluminum ion concentration is 0.02-0.06 mol / L.
4. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: In the aluminum-cobalt mixed solution, the molar ratio of cobalt ions to aluminum ions is 1:0.02-0.
04.
5. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The cobalt salt in the cobalt-aluminum mixed aqueous solution is one or more of cobalt sulfate, cobalt chloride, and cobalt nitrate, and the aluminum salt is one or both of aluminum chloride and aluminum nitrate.
6. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The complexing agent includes one or more of citric acid, ethylenediaminetetraacetic acid and disodium ethylenediaminetetraacetate.
7. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The pH of the mixed solution is 8.5-10.
5.
8. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The drying is vacuum drying at a temperature of 80-100°C.
9. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The screening condition is 200-500 mesh screening.
10. The method for preparing aluminum-doped cobaltous hydroxide according to claim 1, characterized in that: The aluminum-doped cobaltous hydroxide has an aluminum-doped content of 6000-10000 ppm.
Citation Information
Patent Citations
Preparation method of transition metal oxide / sulfide nano composite material
CN106966443A
Preparation method of small-particle-size uniform-aluminum-doped spherical tricobalt tetraoxide
CN109354075A
Preparation method of cobaltous hydroxide
CN109987645A
Preparation method of cobalt hydroxide
CN111559762A
Cobalt oxide porous nanosheets as well as preparation method and application thereof
CN114011412A