Red mud desulfurization slag-based super sulfate cement and preparation method thereof

Through the coordinated use of red mud desulfurization slag and modified red mud desulfurization slag, the hydration rate and the generation of hydration products are changed, which solves the problems of low strength and insufficient adhesion in the early stage of ultrasulfate cement, and improves the overall performance of cement and resource utilization.

CN118930097APending Publication Date: 2024-11-12ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410999238.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing supersulfate cement preparation methods, the early strength is not high, high slag and alkali triggers are required, and the steel slag has weak adhesion to other components, and the composite triggers are high, which increases the preparation cost.

Method used

The red mud desulfurization slag and modified red mud desulfurization slag are used in conjunction with each other. By changing the CaSO4·2H2O component to CaSO4·0.5H2O, the settling time is shortened, and the alkaline components and silicon-aluminum substances in the red mud are used to promote hydration products. Generate, improve early and late intensity.

Benefits of technology

The preparation process is simplified, the early and later strength of ultrasulfate cement is improved, the risks of solid waste storage and pollution are reduced, the anti-chlorine ion penetration performance is improved, and the resource utilization of industrial solid waste is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961098070000041
    Figure BDA0004961098070000041
  • Figure HDA0004961098080000011
    Figure HDA0004961098080000011
  • Figure HDA0004961098080000012
    Figure HDA0004961098080000012
Patent Text Reader

Abstract

The invention belongs to the field of cementing materials, and particularly relates to red mud desulfurization slag-based super sulfate cement and a preparation method thereof. The super sulfate cement is prepared from the following raw materials: red mud desulfurization slag, modified red mud desulfurization slag, red mud and clinker. The super sulfate cement is prepared from some industrial solid wastes, so that the comprehensive utilization of the solid wastes is promoted, and the cost of the super sulfate cement is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cementitious materials, and in particular relates to a red mud desulfurization slag-based supersulfate cement and a preparation method thereof. Background Art

[0002] The cement industry is an important basic industry of my country's national economy and also constitutes the backbone of modern urban construction. With the proposal of "carbon peak and carbon neutrality", reducing energy consumption, reducing harmful gas emissions and improving the utilization rate of industrial waste have become hot topics in the cement industry. Super sulfated cement, as a carbon-friendly "green cementitious material", has received increasing attention.

[0003] CN111302677A discloses a method for preparing supersulfate cement, which reduces the porosity of supersulfate cement and enhances its anti-permeability and anti-carbonation properties. However, the requirements for slag and alkali activators in this scheme are relatively high, and the early strength of the prepared supersulfate cement is not high. CN114735955A discloses a method for preparing desulfurized gypsum-based supersulfate cement, which requires the use of a large amount of sulfate activator, increasing the preparation cost, and the adhesion between steel slag and other components is weak, requiring the use of a composite activator to achieve ideal mechanical properties, and the requirements for the composite activator are relatively high. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a red mud desulfurization slag-based super sulfate cement and to improve the preparation method of the super sulfate cement.

[0005] The technical solution adopted by the present invention is:

[0006] A red mud desulfurization slag-based supersulfate cement, the raw materials and mass percentages are as follows:

[0007] Red mud desulfurization slag 10%-30%;

[0008] Modified red mud desulfurization slag 10%-30%;

[0009] Slag 30%-60%;

[0010] Red mud 10%-20%;

[0011] Clinker 1%-5%;

[0012] The sum of the mass percentages of the above raw materials is 100%.

[0013] The red mud desulfurization slag is waste residue produced after red mud is used for industrial flue gas desulfurization, with a moisture content of ≤5wt%, and main components of CaSO4·2H2O, as well as katoite and cancrinite remaining in the red mud, wherein the content of CaSO4·2H2O is greater than 80%.

[0014] The modified red mud desulfurization slag is red mud desulfurization slag calcined at 170° C. for 4 hours, and the main component is CaSO4·0.5H2O, and the content of CaSO4·0.5H2O is greater than 80%.

[0015] The particle size of the red mud desulfurization slag, modified red mud desulfurization slag and red mud is not less than 100 meshes.

[0016] The clinker is ordinary Portland cement clinker.

[0017] The slag is S95 grade granulated blast furnace slag powder, and its specific surface area is not less than 500m 2 / Kg.

[0018] The red mud is Bayer red mud discharged from alumina production; the red mud contains 10-20wt% CaO, 2-10wt% Na2O and K2O, 20-25wt% Al2O3, 5-15wt% Fe2O3 and 10-25wt% SiO2.

[0019] The method for preparing super sulfated cement comprises the following steps: grinding red mud desulfurized slag, modified red mud desulfurized slag, slag and red mud to achieve the particle size requirement; and mixing red mud desulfurized slag, modified red mud desulfurized slag, slag, red mud and clinker and ball milling (not less than 300 meshes) to obtain red mud desulfurized slag-based super sulfated cement.

[0020] Compared with the prior art, the beneficial technical effects of the present invention are:

[0021] 1. The present invention uses red mud desulfurization slag, modified red mud desulfurization slag, slag, red mud and clinker as raw materials. The raw materials can be mixed and ball-milled during preparation, and the preparation process is very simple.

[0022] 2. The main innovation of the present invention lies in the coordinated use of red mud desulfurization slag and modified red mud desulfurization slag. When red mud desulfurization slag is used alone, the hydration rate of supersulfate cement is slow, resulting in slow strength growth and the disadvantage of low early strength. When a portion of modified red mud desulfurization slag is added, the main component thereof is converted from CaSO4·2H2O to CaSO4·0.5H2O. The solubility of CaSO4·0.5H2O is greater than that of CaSO4·2H2O. CaSO4·0.5H2O will produce self-hydration when it meets water. Adding it to supersulfate cement will greatly shorten the setting time of supersulfate cement and improve the early strength of supersulfate cement. At the same time, the activity of katoite and cancryogenite in the modified red mud desulfurization slag increases after calcination, and can participate in promoting the formation of C-(A)-SH gel, a hydration product of supersulfate cement, further promoting the hydration of supersulfate cement and also improving the early strength.

[0023] 3. The addition of red mud in the present invention has two functions. First, the alkaline components therein act as alkaline activators to disintegrate the slag. Specifically, Na2O and K2O in the red mud can destroy the slag structure and promote the disintegration of the slag glass network. Second, a large amount of siliceous and aluminous substances (such as SiO2 and Al2O3) in the red mud can be disintegrated under the action of clinker to generate C-(A)-SH gel, a hydration product of supersulfate cement, which can improve the later strength of supersulfate cement.

[0024] 4. The present invention combines the resource utilization of industrial solid waste with the preparation of cementitious materials, effectively reduces the risk of solid waste storage and pollution, and promotes the comprehensive utilization of solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Appearance of red mud desulfurization slag-based super-sulfate cement test block.

[0026] Figure 2 Scanning electron microscope image of the red mud desulfurization slag-based super-sulfated cement specimen after crushing. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are described below in conjunction with examples. However, the following examples are only used to illustrate the present invention in detail and are not intended to limit the scope of the present invention in any way.

[0028] In the following embodiments:

[0029] Example: Red mud desulfurization slag is the waste residue produced after red mud is used for industrial flue gas desulfurization, with a moisture content of ≤5wt%, and the main component is CaSO4·2H2O, of which the content of CaSO4·2H2O is greater than 80%. There is also a small amount of katoite Ca3Al2(SiO4)(OH)8 and cancrinite Na6Ca2Al6Si6O in the red mud. 24 The modified red mud desulfurization slag is red mud desulfurization slag calcined at 170°C for 4 hours, and the main component is CaSO4·0.5H2O, and the content of CaSO4·0.5H2O is greater than 80%. The particle size of red mud desulfurization slag, modified red mud desulfurization slag and red mud is 100 mesh.

[0030] Table 1 Raw material dosage of each embodiment

[0031]

[0032] The method for preparing super sulfated cement comprises the following steps: grinding red mud desulfurized slag, modified red mud desulfurized slag, slag and red mud to achieve the particle size requirement (not less than 100 mesh); mixing red mud desulfurized slag, modified red mud desulfurized slag, slag, red mud and clinker and ball milling (not less than 300 mesh) to obtain red mud desulfurized slag-based super sulfated cement.

[0033] Effect experiment:

[0034] Referring to GB / T 17671-1999 “Test method for strength of cement mortar (ISO method)”, the compressive strength of each group of cement in Table 1 at 1d, 3d, 7d and 28d was tested. The results are shown in Table 2.

[0035] Table 2 Compressive strength of each embodiment (MPa)

[0036] Example 1d 3d 7d 28d 1 14.53 17.50 25.60 42.92 2 17.24 19.42 26.10 44.05 3 16.12 18.62 24.62 44.28 4 18.29 19.76 26.15 45.72 5 16.26 19.58 23.80 43.48 6 16.34 18.34 22.02 44.85 7 17.25 17.89 22.72 45.60 8 5.25 12.18 20.17 35.82 9 6.71 13.00 21.62 38.17 10 3.42 9.67 17.95 34.78

[0037] As can be seen from Table 2, when modified red mud desulfurization slag is added in a specific ratio in Examples 1-7, the strength of super sulfate cement is improved, especially the early strength (1d and 3d), and the effect of Example 4 is the best. When there is no modified red mud desulfurization slag or the addition amount of modified red mud desulfurization slag is too low, the early strength is not significantly improved. When the addition amount of modified red mud desulfurization slag is too high, the internal structure of the cement is unevenly developed due to the short setting time, which leads to a decrease in strength.

[0038] According to the national standard GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", Examples 1-10 (28d) were tested for resistance to chloride ion penetration. The results are shown in Table 3.

[0039] Example 1 2 3 4 5 6 7 8 9 10 Electric flux / C 119 106 107 97 121 126 119 326 358 432

[0040] As shown in Table 3, the supersulfate cement prepared in Examples 1-7 exhibits good resistance to chloride ion penetration, indicating that the supersulfate cement with a certain amount of modified red mud desulfurization slag added has excellent resistance to chloride ion penetration. As can be seen from the data of Examples 8-10, when no or a small amount or too much modified red mud desulfurization slag is added, the resistance to chloride ion penetration of supersulfate cement decreases.

[0041] The appearance of the supersulfate cement prepared in Example 4 after hydration and curing is shown in the figure below: Figure 1 As shown, the color is gray-brown. The scanning electron microscope image after crushing is as follows Figure 2 As shown by Figure 2 The main hydration products of supersulfated cement, ettringite (AFt) and C-(A)-SH gel, can be observed. The network-like C-(A)-SH gel tightly wraps AFt to form a relatively dense overall structure. AFt and C-(A)-SH gel are intertwined and work together to improve the density of the paste structure.

[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A red mud desulfurization slag-based supersulfate cement, characterized in that: The raw materials and mass percentages are as follows: Red mud desulfurization slag 10%-30%; Modified red mud desulfurization slag 10%-30%; Slag 30%-60%; Red mud 10%-20%; Clinker 1%-5%; The sum of the mass percentages of the above raw materials is 100%.

2. The supersulfate cement according to claim 1, characterized in that: The red mud desulfurization slag is waste residue generated after red mud is used for industrial flue gas desulfurization, with a moisture content of ≤5wt%, and a main component of CaSO4·2H2O, wherein the content of CaSO4·2H2O is greater than 80%.

3. Supersulfate cement according to claim 1 or 2, characterized in that: The modified red mud desulfurization slag is red mud desulfurization slag calcined at 170° C. for 4 hours, and the main component is CaSO4·0.5H2O, and the content of CaSO4·0.5H2O is greater than 80%.

4. Supersulfate cement according to claim 1 or 2, characterized in that: The particle size of the red mud desulfurization slag, modified red mud desulfurization slag and red mud is not less than 100 meshes.

5. Supersulfate cement according to claim 1 or 2, characterized in that: The clinker is ordinary Portland cement clinker.

6. A method for preparing supersulfated cement according to any one of claims 1 to 5, characterized in that: The red mud desulfurization slag, modified red mud desulfurization slag, slag and red mud are ground to meet the particle size requirements; the red mud desulfurization slag, modified red mud desulfurization slag, slag, red mud and clinker are mixed and ball-milled to obtain the red mud desulfurization slag-based super sulfate cement.

Citation Information

Patent Citations

  • Supersulfate cement and preparation method thereof

    CN111302677A

  • Desulfurized gypsum-based super sulfate cement and preparation method thereof

    CN114735955A