High-adaptability cement clinker grinding aid and preparation method thereof
Through the combination technology of dispersant and defect inducer, a high-adaptive cement clinker aid was prepared, which solved the problems of low grinding efficiency of alcohol amine aid and unstable product quality, and achieved high fineness of cement particles and strength enhancement, suitable for a wider range of grinding assistance.
Patent Information
- Application Number
- CN202411059583.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cement agitators have problems with low grinding efficiency and unstable product quality, especially the alcohol amine agitators have problems with difficult components and poor product stability.
Polyether monomers are prepared by reacting alcohol heads with epoxy monomers and formulated with initiators, chain transfer agents and ether substances in a 2:1:3 mass ratio. Ingredients dispersant, combined with amine heads and cyclic monomers to prepare defect inducers, and finally combined into high-adaptive cement clinker aids, with small molecular weight and strong dispersion, which can effectively improve the specific surface area and fineness of cement particles .
It significantly improves the fineness and specific surface area of cement particles, enhances the hydration strength, and shows a wider grinding effect at lower dosage, avoiding the adsorption barrier of traditional grinding agents and component incompatibility problems. .
Smart Images

Figure BDA0004977458230000041 
Figure BDA0004977458230000051 
Figure BDA0004977458230000052
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, in particular to a highly adaptable cement clinker grinding aid and a preparation method thereof. Background Art
[0002] Cement grinding aid is an additive that acts during the grinding process. It is generally composed of surfactants. It adsorbs on the surface of cement particles through its polar groups, reduces the surface tension of the particles, and repels the electrostatic repulsion between particles, thereby weakening the phenomenon of particle agglomeration, ultimately achieving the purpose of improving grinding efficiency and optimizing product quality.
[0003] CN202310108726.6 discloses a method for preparing a high-efficiency cement grinding aid. The grinding aid uses alkali lignin as the main raw material, and improves its grinding aid and enhancement performance for cement clinker and mixed materials through modification; the ammonium persulfate oxidation modification method is used to reduce the relative molecular mass of alkali lignin, increase the polar groups in its molecules, and prepare a high-efficiency cement grinding aid. Lignin derivative grinding aids have been proven to have a weak grinding aid effect because their sulfonic acid group content is low, and their molecular weight distribution is wide and their molecular structure is generally unreasonable, resulting in weak adsorption capacity. This invention has a certain positive effect on lignin derivative grinding aids through modification.
[0004] CN202310136969.0 discloses a method for preparing a novel cement grinding aid. A thiol addition reaction is performed between triethanolamine maleate, 1,6-hexyldithiol, oleylamine, and glycerol allyl ether. The invention adopts a more traditional alcoholamine system, and its molecular structure contains a fatty chain segment, a negatively charged group, and an alcoholamine group, which plays a certain dispersing and adsorbing role. The grinding aid neutralizes the residual charge on the particle surface through the adsorption of the negatively charged group and the positive charge on the particle surface to prevent the particle from healing. The role of the fatty chain forging is that when the polymer is adsorbed on the particle surface, it can play the effect of accelerating the flow rate, further wet the interface, and prevent the phenomenon of excessive grinding from occurring. When the proportions of various functional groups in the molecular structure are appropriate, it can play a good dispersing role and prevent the powder from running coarse.
[0005] CN201911162939.7 discloses a method for preparing a cement grinding aid. The grinding aid is polymerized under appropriate conditions according to a certain molar ratio of polyamine monomers, unsaturated carboxylic acid esters, diluents, amino polyethers, and alkylene oxides. Under suitable synthesis conditions, a polymer grinding aid with good grinding aid effect and high storage stability can be prepared according to the optimal molar ratio. The amine group in the structure chelates with the metal elements in the clinker by providing electron pairs to achieve the purpose of adsorption, and the amino polyether side chain disperses the particles through steric hindrance, thereby ultimately improving the grinding efficiency.
[0006] The above research work shows that cement grinding aids, whether prepared in the form of monomer compounding or by free radical polymerization of monomers, have a positive effect on the grinding effect. Grinding aids of alcohol amine compounding systems, represented by alcohol amine systems, often have the problem of incompatible components and poor product stability; the selection of monomers for polymer grinding aids requires a lot of research, and the molar ratio between monomers also needs to be finely adjusted. Summary of the invention
[0007] The invention provides a highly adaptable cement clinker grinding aid and a preparation method thereof, which can solve the problems of low grinding efficiency and unstable product quality of alcohol amine grinding aids. The technical scheme of the invention is as follows, and the parts hereinafter are parts by mass.
[0008] The highly adaptable cement clinker grinding aid of the present invention is characterized in that it is compounded by the prepared dispersant, defect inducer, and polymer polyol in a mass ratio of 2:1:3, and the following parts are all parts by mass;
[0009] The dispersant is prepared by 37.89-57.07 parts of alcohol head, 1.0-2.2 parts of catalyst, 116.65-125.48 parts of cyclic monomer at 120-130° C., and 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to prepare A liquid, and 138.97-165.90 parts of ether substance, 3.2-7.9 parts of reducing agent and water to prepare B liquid are added dropwise to the polyether monomer at 55-65° C. to obtain;
[0010] The defect inducing agent is obtained by polymerizing 104.96 to 185.26 parts of amine heads, 1.0 to 2.2 parts of catalysts and 114.75 to 195.05 parts of cyclic monomers at 90-120°C.
[0011] The preparation method of the highly adaptable cement clinker grinding aid of the present invention is as follows:
[0012] (1) Preparation of dispersant
[0013] Step 1: Add 37.89-57.07 parts of alcohol head and 1.0-2.2 parts of catalyst into the autoclave, replace with nitrogen several times, start to evacuate to the gauge pressure -0.1MPa, then heat to 120-130°C to start dehydration for 1-2h, then cool to 115°C to start continuous and uniform introduction of 116.65-125.48 parts of cyclic monomer, control the pressure to be less than 0.4MPa, keep warm at 110-120°C for 1.5-2.5h to react to negative pressure, cool and discharge to obtain polyether monomer;
[0014] Step 2: Add the prepared polyether monomer to the reaction kettle, heat it to 55-65°C by water bath heating, and then keep it warm; prepare 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to make liquid A; prepare 138.97-165.90 parts of ether substance, 3.2-7.9 parts of reducing agent, 0.5-1.0 parts of alcohol head and water to make liquid B; drip liquid A and liquid B at the same time, wherein liquid A is dripped for 2-2.5 hours, and liquid B is dripped for 1.5-2 hours; after liquid A is dripped, keep it warm for 1 hour, add 5.9-9.4 parts of neutralizer at one time, and add water to 1000 parts to obtain a dispersant mother liquor with a concentration of 30wt%. The several parts of polyether monomer prepared in step 1 are adjusted in a certain proportion according to the required amount in step 2, so as to control the concentration of the dispersant mother liquor obtained by the reaction to be always controlled at 30%, which reduces the workload for subsequent compounding and other work.
[0015] (2) Preparation of defect-inducing agents
[0016] Step 1: Add 104.96-185.26 parts of amine heads into a high-pressure reactor, raise the temperature to 120°C while evacuating, and the pressure in the reactor is 0.2-0.3MPa. The material in the reactor is sucked out from the reactor and then sprayed into the reactor from the top. At the same time, add cyclic monomers. After a period of circulation, cool to 90-100°C.
[0017] Step 2: Add 1.0 to 2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1 MPa, then raise the temperature to 120°C. Start to introduce the remaining cyclic monomers into the reactor, introduce a total of 114.75 to 195.05 parts of cyclic monomers into the reactor, control the pressure to be less than 0.4 MPa, keep circulating spray for 2.0 to 2.5 hours after all the cyclic monomers are introduced into the reactor, keep warm for 1 hour after the reaction is completed, add 5.9 to 9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a defect inducing agent mother liquor with a concentration of 30wt%.
[0018] (3) Preparation of highly adaptable cement clinker grinding aid
[0019] The prepared dispersant, defect inducer and polymeric polyol are compounded in a mass ratio of 2:1:3, and water is added to 1000 parts to obtain the highly adaptable cement clinker grinding aid mother liquor with a mass concentration of 50wt%.
[0020] Preferably, the alcohol head is (E)-4-hexen-1-ol.
[0021] Preferably, the catalyst is one of sodium hydroxide, sodium methoxide and potassium hydroxide, and potassium hydroxide is most preferred.
[0022] Preferably, the cyclic monomer is ethylene oxide.
[0023] Preferably, the initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate, and dihexyl peroxydicarbonate, and dihexyl peroxydicarbonate is most preferred; the chain transfer agent is one of thioglycolic acid, mercaptoethanol, and mercaptopropionic acid, and mercaptopropylamine is most preferred; the ether substance is one of diethylene glycol monoallyl ether and polypropylene glycol, and polypropylene glycol is most preferred.
[0024] Preferably, the amine head is N-methyl-allylamine; the reducing agent is sodium hypophosphite; and the neutralizing agent is potassium carbonate.
[0025] Preferably, the alcohol-ether ratio is 2.1-3:1, most preferably 2.8:1.
[0026] Preferably, the polymeric polyol is composed of several of ethylene glycol, glycerol, trimerpropylene glycol and triethanolamine.
[0027] Preferably, the ratio of the dispersant, the defect inducer and the polymeric polyol is 2:1:3.
[0028] The present invention is based on the functional design of polymers based on the reaction of the terminal hydroxyl group of the alcohol head with the epoxy monomer. The alcohol head and the epoxy group are etherified to synthesize a low molecular weight polymer of about 5300 to 7900. The epoxy material is selected from ethylene oxide and propylene oxide. The number of methyl groups is adjusted by adjusting the grafting ratio of ethylene oxide and propylene oxide. Studies have found that methyl groups have a certain effect of improving the particle size. The number of methyl groups is adjusted according to the ratio of the two epoxides, so that the polymer can fully exert its effect of improving the particle size and fineness.
[0029] The defect inducer is prepared by reacting N-methyl-allylamine with epoxide to prepare a low molecular weight substance of 120 to 200. The terminal amine group in the molecular structure has the same function as the alcohol amine, that is, the amine group can give out electron pairs and combine with the aluminum in tricalcium silicate and tetracalcium aluminoferrite in the clinker, thus destroying the surface structure of the clinker particles and inducing more defects in the particles.
[0030] The composite use of dispersant and defect inducing agent ensures that the grinding aid improves the particle specific surface area. At the same time, the high dispersibility of the polyether side chain prevents the agglomeration of particles and accelerates the flow rate of materials in the mill. Furthermore, the molecular weight of this grinding aid is smaller than that of traditional polymer grinding aids, which is conducive to the free movement of components between material layers and their effects, and has a wider range of grinding aid effects on cement clinker.
[0031] The beneficial effects of the present invention are as follows:
[0032] 1. The dispersed components of the grinding aid provided by the present invention have a relatively small molecular weight, concentrated in the range of about 5000 to 8000, and can be better freed in the narrow gaps between the clinker particles, and have a wider range of action.
[0033] 2. The dispersant component in the grinding aid provided by the present invention has a relatively weak adsorption capacity, while the clinker is a grindable material with a relatively high surface activity, so the dispersant component will not be ineffective due to adsorption obstruction.
[0034] 3. The defect inducing agent component in the grinding aid provided by the present invention can effectively combine with the aluminum in the clinker, thereby leaving defects on the particle surface. The polymer hydrophobic groups are easy to extend into the cracks, thereby hindering the agglomeration of particles and improving the particle fineness. At the same time, the defects on the clinker surface provide it with a larger specific surface area, which also has a certain promoting effect on hydration. DETAILED DESCRIPTION
[0035] The applicant will further explain the technical solutions and beneficial effects of the present invention in detail in conjunction with specific embodiments, but it should be understood that the following embodiments should not be construed as limiting the scope of protection requested by the claims of this application to any extent.
[0036] The grinding aids obtained in each embodiment according to the method are used in cement grinding for performance testing, and the duration is 30 minutes. The proportions of cement used in the test are exactly the same, and the cement mass proportions are: 76% clinker, 5% gypsum, 8% slag, and 11% fly ash. The grinding aid doping amount of each test group is 0.03%; the commercially available grinding aid (Hongxin HX-ZQY grinding aid) is 0.05%. The strength of the cement mortar after grinding of each embodiment and the comparative example is tested according to the method described in the national standard GB / T17671-1999, and the specific surface area of the cement after grinding of each embodiment and the comparative example is measured by the FBT-9 cement Blaine fully automatic specific surface area measuring instrument, and the 45μm sieve residue of the cement after grinding of each embodiment and the comparative example is measured by the FSY-150 cement fineness negative pressure sieve analyzer; the cement obtained by grinding is mixed with machine-made sand and water to prepare a mortar test block, and the compressive strength test is carried out. Particle size distribution: measured by Mastersizer3000 laser particle size analyzer. The results are shown in Tables 3 and 4.
[0037] Table 1 Preparation raw material composition of highly adaptable grinding aid
[0038]
[0039]
[0040] Table 2 Preparation process of highly adaptable cement clinker grinding aid
[0041]
[0042] Table 3 Grinding aid performance test results
[0043]
[0044] Table 4 Particle size distribution test results
[0045]
[0046] As shown in Table 3, compared with commercial grinding aids, the cement grinding aid prepared by the present invention has a significant effect on improving the cement particle specific surface area when the dosage is less, and the particle fineness is slightly improved compared with the commercial grinding aid; the improvement of hydration strength is very obvious, and compared with the commercial grinding aid, the enhancement effect in the early and late stages is very obvious. Combined with the data of particle size distribution in Table 4, it can be proved that the grinding aid prepared by the present invention can greatly improve the volume fraction of fine particles, which is specifically manifested in that the content of particles of 0 to 32 μm is significantly higher than that of commercial grinding aids.
[0047] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly adaptable cement clinker grinding aid, characterized in that: The prepared dispersant, defect inducing agent and polymerized polyol are compounded in a mass ratio of 2:1:3, and the following parts are all parts by mass; The dispersant is prepared by 37.89-57.07 parts of alcohol head, 1.0-2.2 parts of catalyst, 116.65-125.48 parts of cyclic monomer at 120-130° C., and 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to prepare liquid A, and 138.97-165.90 parts of ether substance, 3.2-7.9 parts of reducing agent and water to prepare liquid B to prepare liquid B at 55-65° C. to obtain; The defect inducing agent is obtained by polymerizing 104.96-185.26 parts of amine heads, 1.0-2.2 parts of catalysts and 114.75-195.05 parts of cyclic monomers at 90-120°C.
2. The method for preparing the highly adaptable cement clinker grinding aid according to claim 1, characterized in that The parts are all parts by mass, comprising the following steps: (1) Preparation of dispersant Step 1: Add 37.89-57.07 parts of alcohol head and 1.0-2.2 parts of catalyst into the autoclave, replace with nitrogen several times, start to evacuate to the gauge pressure -0.1MPa, then heat to 120-130°C to start dehydration for 1-2h, then cool to 115°C and start to continuously and uniformly introduce 116.65-125.48 parts of cyclic monomer, control the pressure to be less than 0.4MPa, keep warm at 110-120°C for 1.5-2.5h to react to negative pressure, cool and discharge to obtain polyether monomer; Step 2: Add the prepared polyether monomer into the reaction kettle, heat it to 55-65°C in a water bath and then keep it warm; prepare liquid A by adding 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water; prepare liquid B by adding 138.97-165.90 parts of ether substance, 3.2-7.9 parts of reducing agent, 0.5-1.0 parts of alcohol head and water; add liquid A and liquid B at the same time, wherein liquid A is added for 2-2.5 hours and liquid B is added for 1.5-2 hours; after adding liquid A, keep it warm for 1 hour, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a dispersant mother solution with a concentration of 30wt%; (2) Preparation of defect inducers Step 1: Add 104.96~185.26 parts of amine head into the autoclave, raise the temperature to 120℃ while evacuating, the pressure in the autoclave is 0.2~0.3MPa, the material in the autoclave is sucked out from the autoclave and then sprayed into the autoclave from the top, and the cyclic monomer is added at the same time. After a period of circulation, cool to 90~100℃; Step 2: Add 1.0-2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1MPa, then raise the temperature to 120°C. Start to introduce the remaining cyclic monomers into the reactor, introduce a total of 114.75-195.05 parts of cyclic monomers into the reactor, control the pressure to be less than 0.4MPa, keep circulating spray for 2.0-2.5h after all the cyclic monomers are introduced into the reactor, keep warm for 1h after the reaction is completed, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a defect inducing agent mother liquor with a concentration of 30wt%; (3) Preparation of highly adaptable cement clinker grinding aid The prepared dispersant, defect inducer and polymeric polyol are compounded in a certain proportion and water is added to 1000 parts to obtain the highly adaptable cement clinker grinding aid mother liquor with a concentration of 50%. The highly adaptable cement clinker grinding aid mother liquor is diluted at a ratio of 1:29 to obtain the highly adaptable cement clinker grinding aid working solution, and its usage dosage is 0.03%.
3. The method according to claim 2, characterized in that The alcohol head is (E)-4-hexen-1-ol.
4. The method according to claim 2, characterized in that: The catalyst is one of sodium hydroxide, sodium methoxide and potassium hydroxide.
5. The method according to claim 2, characterized in that: The cyclic monomer is ethylene oxide.
6. The method according to claim 2, characterized in that The initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate and dihexyl peroxydicarbonate; the chain transfer agent is one of thioglycolic acid, mercaptoethanol and mercaptopropionic acid; and the ether substance is one of diethylene glycol monoallyl ether and poly(1,2-propylene glycol).
7. The method according to claim 2, characterized in that The amine head is N-methyl-allylamine; the reducing agent is sodium hypophosphite; and the neutralizing agent is potassium carbonate.
8. The method according to claim 2, characterized in that: The alcohol-ether molar ratio is 2.1-3:
1.
9. The method according to claim 2, characterized in that: The polymeric polyol is composed of several of ethylene glycol, glycerol, trimeryl glycol and triethanolamine.
10. The method according to claim 2, characterized in that The mass ratio of the dispersant, the defect inducer and the polymerized polyol is 2:1:3.
Citation Information
Cited By
Cement grinding aid with high adsorption capacity and preparation method thereof
CN121203103A