Colored micro-surfacing concrete and preparation method thereof
By using modified emulsified asphalt and sandblasting treatment technology in color micro surface concrete, the problems of poor visualization effect and poor color durability at night are solved, the durability and anti-slip performance of the pavement materials are improved, and the Preparation process improves driving safety.
Patent Information
- Application Number
- CN202411122838.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
The existing colored asphalt pavement materials have poor night visualization effects, poor color durability, complex preparation process, poor material performance, and insufficient pavement durability.
Using colored micro-surface concrete, sand particles, stained glass, cement, steel slag powder, red mud and modified emulsified asphalt are mixed in a specific proportion, and cationic surfactant and vulcanized crosslinker are added to sandblasting. Improve the roughness of the glass and form modified emulsified asphalt to enhance the stability and durability of the concrete.
The night visualization effect, color durability, simplification of preparation process and improvement of material performance of colored pavements is achieved, ensuring the anti-slip, wear resistance and durability of the pavement, alleviating the driver's visual fatigue and improving safety.
Smart Images

Figure CN118930182A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of colored asphalt pavement, and in particular to a colored micro-surfacing concrete and a preparation method thereof. Background Art
[0002] The main types of domestic road surfaces are asphalt or cement. However, the traditional road surface has a single color, and long-term driving can easily cause visual fatigue. In addition, it is difficult to provide a clear sense of road boundary vision when the lights illuminate the road surface and vehicles meet during night driving, which greatly threatens the safety of drivers and pedestrians. With the development of industry and the improvement of people's living standards, colored glass products are gradually accepted and used by people. However, the recycling of waste colored glass requires manual or machine color selection, which is a complicated process and difficult to ensure quality control. The use of micro-surfacing maintenance technology to apply colored glass to the road surface can not only effectively solve the problems of waste glass pollution and natural aggregate shortage, slow down the occurrence of road diseases and improve the roadscape viewing, but also relieve driving fatigue, improve the nighttime visualization of the road surface, and play a safety warning effect.
[0003] At present, there are many technologies for color asphalt pavement. For example, Chinese invention patent CN115557731A discloses a modified color asphalt binder, which is applied to micro-surfacing asphalt pavement. It uses color powder, light oil component, anti-aging agent, petroleum resin, stabilizer, etc. to prepare modified color asphalt. Since its color is mainly provided by color powder, and its aging resistance and weather resistance are poor, this technology is limited by the influence of environment and time. Chinese invention patent CN107555844A discloses a luminous color asphalt concrete and preparation method, which is prepared based on asphalt, emulsifier, glass microbeads, aluminum powder, reflective agent, tackifier, stabilizer, etc., and its nighttime visualization effect is limited. Color additives such as reflective agents are greatly affected by ultraviolet radiation. The surface of traditional glass is smooth, and it reflects mirror-emitted light, which will cause the driver to be dazzled and dizzy, and feel uncomfortable. In addition, it has poor compatibility with asphalt materials, and it is difficult to ensure that the asphalt pavement has a long-term color luminous effect. Chinese invention patent CN110540378A discloses a colored pavement material composed of glass particles. The sintering process of the glass granulation is complex and the precision is strictly controlled. Since white glass is used, its reflectivity is poor and the nighttime visualization effect is limited.
[0004] The information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art known to those skilled in the art. Summary of the invention
[0005] The first purpose of the present invention is to provide a colored micro-surfacing concrete to solve the problems of poor nighttime visualization, poor color durability, complex preparation process, poor material performance and insufficient pavement durability of current colored asphalt pavement materials.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0008] The colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10-20:20-30:70-80:3-5:1-3:1-2:3-5:1-2;
[0009] Modified emulsified asphalt is emulsified asphalt modified by cationic surfactant and vulcanized crosslinking agent. The mass ratio of cationic surfactant is 2‰~5‰ of emulsified asphalt, and the mass ratio of vulcanized crosslinking agent is 2‰~3‰ of emulsified asphalt. The addition of cationic surfactant can improve the stability and adhesion of emulsified asphalt, which is conducive to the uniformity and durability of concrete. The role of vulcanized crosslinking agent is to enhance the structural stability of emulsified asphalt and improve its performance in concrete.
[0010] In the color micro-surfacing concrete prepared by the present invention, during the mixing process, the granular materials such as crushed stone, sand, and colored glass play a filling and supporting role in the concrete. After the cement is solidified as a cementitious material, the particles are fixed together to form the basic structure of the concrete. By adding the colored glass to the concrete according to the percentage of different particle sizes, the particles can be evenly distributed. The coarse-grained colored glass fills the larger voids, increasing the compactness and strength of the concrete; while the fine-grained colored glass fills the smaller voids, improving the overall density and impermeability of the concrete. Red mud can improve the durability and impermeability of the concrete. Red mud reacts with cement to form a composite cementitious material, which further enhances the structural stability and durability of the concrete. It can fill the tiny voids in the concrete and improve the compactness and wear resistance of the concrete. The modified emulsified asphalt reacts with cement to form a composite cementitious material, which further enhances the structural stability and durability of the concrete. The components work synergistically with each other to improve the performance and durability of the concrete.
[0011] Preferably, in the colored glass, the mass percentage of the maximum nominal particle size is as follows:
[0012] 2.36mm~4.75mm coarse particle size colored glass, 20%~40%;
[0013] 0mm~2.36mm fine-grained colored glass, 60%~80%. By adding colored glass to concrete according to the percentage of different particle sizes, the particles can be evenly distributed. Coarse-grained colored glass can fill larger voids in concrete, increase the compactness and strength of concrete; while fine-grained colored glass can fill smaller voids, improve the overall density and impermeability of concrete. In addition, the use of coarse and fine-grained colored glass can make the micro-surfacing road surface have excellent and stable anti-skid and wear-resistant properties. Coarse-grained colored glass forms bulges on the road surface, increases the friction of the road surface, and improves the stability and safety of vehicles when driving; fine-grained colored glass fills tiny voids, increases the compactness and wear resistance of the road surface, and extends the service life of the road surface.
[0014] Preferably, the colored glass is obtained by roughening waste glass; the colored glass is mainly waste glass (any one or more combinations of green material, yellow-black material, white magnetic material, red-blue material). Green material refers to green and dark glass, including discarded wine bottles, vases, cosmetic bottles, etc.; yellow-black material refers to black and yellow glass, including discarded yellow medicine bottles and reagent bottles; white magnetic material refers to opaque glass, including cosmetic bottles and white magnetic lampshades; red-blue material refers to red and blue glass, including red and blue glass bottles or glass doors and windows, etc.; after the waste glass is roughened, microscopic bumps and textures will be formed on its surface, which helps to improve the bonding strength between the colored micro-surface concrete and the cement matrix and enhance the overall performance and durability of the concrete. At the same time, the hardness and compressive strength of the colored glass can also provide additional reinforcement for the concrete.
[0015] The Mohs hardness of colored glass is between 5.4 and 6.5; coarse and fine colored glass with a Mohs hardness of 5.4-6.5 has rich angularity, which increases the structural depth of the micro-surfacing pavement material and improves the anti-skid performance. In addition, discarded colored glass is mostly made of sintered white glass and metal colloid particles, not colored on the glass surface. Compared with white glass, it has better reflectivity, so its color has natural weather resistance and is not affected by the environment and time. The use of coarse and fine particle size colored glass to prepare micro-surfacing can not only ensure the nighttime visualization effect, color durability, and preparation process of the micro-surfacing pavement, but also make the micro-surfacing pavement have excellent and stable anti-skid and wear resistance.
[0016] The roughening process of stained glass includes:
[0017] Place the broken colored glass in the sandblasting room, the sandblasting pressure is 0.2MPa~0.6MPa, and the sandblasting speed is 30cm 2 / min~50cm 2 / min, the sandblasting time is 4min~6min, and the polishing value of the colored glass is 36~42. After sandblasting, microscopic concave-convex and texture are formed on the surface of the colored glass, which improves the mechanical bonding between the colored glass and the concrete matrix. This ensures that the colored glass can be better combined with the concrete, and enhances the durability and stability of the colored micro-surface concrete. On this basis, the microscopic concave-convex structure on the surface of the colored glass can increase the filling speed of cement and colored glass, and accelerate the solidification and hardening process of concrete. It helps to improve construction efficiency, shorten construction period and reduce construction costs.
[0018] Preferably, the particle size of the crushed stone is 4.75 mm to 9.5 mm, and the crushed stone includes any one or more combinations of diabase, andesite, limestone, and basalt. The crushed stone is hard and wear-resistant, providing a high-wear-resistant and high-strength skeleton structure for the micro-surfacing.
[0019] Preferably, the particle size of the sand is 0.075 mm to 1.12 mm, and the sand includes any one or more combinations of silica sand, glass sand, and corundum. Sand plays the role of filler and aggregate in concrete, and its suitable particle size range can fill the gaps between cement particles and increase the compactness of concrete. At the same time, the addition of sand can increase the strength and compression resistance of concrete, and improve the bearing capacity and durability of concrete.
[0020] Preferably, the cement is P·O 42.5 ordinary Portland cement.
[0021] Preferably, the steel slag powder is made by grinding converter steel slag, with a purity of 90% to 100% and a particle median diameter of 0.8um to 12um. As a supplementary material, the steel slag powder can fill microscopic voids in concrete, improve the compactness and firmness of concrete, and thus improve the crack resistance and durability of concrete. In particular, the characteristics of its fine particles can fill tiny cracks, effectively prevent the expansion of cracks, and extend the service life of concrete.
[0022] Preferably, the red mud is steel smelting red mud, wherein the iron oxide content is 35% to 65% and the particle median diameter is 0.075 mm to 1.12 mm. It can fill the microscopic voids in the concrete, increase the density and firmness of the concrete, and thus improve the compression resistance and durability of the concrete. The components such as iron oxide have good oxidation resistance and weather resistance, can effectively resist the erosion of the external environment, and delay the aging and corrosion process of the concrete.
[0023] As a preferred method, the preparation method of modified emulsified asphalt comprises:
[0024] S11: Add the vulcanized crosslinking agent to water in a ratio of 1:1, adjust the pH value to 2-3 with concentrated hydrochloric acid, and then heat to 70-76°C while stirring to fully dissolve it;
[0025] S12 sends the asphalt heated to 140-150°C and the vulcanized cross-linking agent in proportion into the colloid mill for emulsification, ensuring that the vulcanized cross-linking agent is fully dispersed in the asphalt, thereby improving the stability and performance of the modified emulsified asphalt.
[0026] S13 adds cationic surfactants in proportion at the outlet of emulsified asphalt, and then uses a stirrer to fully mix them in the emulsified asphalt storage to obtain modified emulsified asphalt; the cationic surfactants in the process can further improve the stability and dispersibility of the emulsified asphalt, ensuring its uniform distribution and excellent performance in the concrete.
[0027] Preferably, the cationic surfactant is hexadecyltrimethylammonium chloride; the vulcanized crosslinking agent is diisocyanate. Hexadecyltrimethylammonium chloride can reduce the surface tension in the emulsified asphalt, making it easier for the asphalt particles to disperse in the water phase, thereby improving the emulsification stability. A surfactant film is formed between the asphalt particles and the water phase, which helps to prevent the agglomeration and precipitation of the asphalt particles and improve the stability of the emulsified asphalt. It can also enhance the adhesion between the asphalt particles and the concrete particles, and improve the mechanical properties and durability of the concrete. Diisocyanate can undergo a cross-linking reaction with the sulfur-containing groups in the asphalt to form a cross-linking structure, which increases the connectivity between the asphalt molecules. The formation of the cross-linking structure makes the modified emulsified asphalt have higher viscosity and stickiness, can better adhere to the aggregate surface, and improve the water resistance and impermeability of the concrete. Diisocyanate can also inhibit the aging process of asphalt, delay its oxidation and degradation in the environment, thereby extending the service life of the concrete.
[0028] The second object of the present invention is to provide a method for preparing colored micro-surfacing concrete, which has the same technical effect.
[0029] In order to achieve the above object, the technical solution adopted by the present invention is:
[0030] A method for preparing colored micro-surfacing concrete, comprising:
[0031] According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder and red mud are mixed for 40s-50s until uniform, and then water is added and mixed for 35s-45s until it is wet. The addition of water can activate the hydration reaction of cement, promote the hardening and curing process of concrete, and make the mixture easier to plastically deform, which is conducive to subsequent construction and molding. Then add modified emulsified asphalt and mix for 35s-50s to obtain a uniform colored micro-surface concrete. The addition of modified emulsified asphalt can improve the bonding strength and water resistance of concrete, enhance the durability and stability of concrete, and thus ensure the quality and performance of colored micro-surface concrete.
[0032] The beneficial effects of the present invention are:
[0033] The waste colored glass in the present invention is mostly made of white glass and metal colloidal particles sintered, not colored on the glass surface, and has better reflectivity than white glass, so its color has natural weather resistance and is not affected by the environment and time. The use of coarse and fine particle size colored glass to prepare micro-surface can not only ensure the nighttime visualization effect, color durability, and preparation process of the micro-surface road surface, but also make the micro-surface road surface have excellent and stable anti-skid and wear-resistant properties.
[0034] The present invention adopts a sandblasting process to roughen broken glass, and applies it together with sand particles to micro-surfacing concrete; cement, steel slag powder, and red mud are used as inorganic gelling materials to provide an anti-stripping effect for the micro-surfacing bonding layer; cationic surfactants and vulcanized cross-linking agents provide adhesion and durability for the emulsified asphalt after demulsification.
[0035] On the one hand, the roughened colored glass used in the present invention not only enhances the adhesion between the substrate and the binder, but also realizes the resource utilization of waste glass, alleviates the pressure it causes to the environment, and avoids the mining of natural stones to protect natural resources; on the other hand, the application of roughened colored glass on asphalt pavement provides diffusely reflected flexible light, which can relieve the driver's visual fatigue. At the same time, the road surface has good nighttime visualization characteristics. Under weak light, a large number of soft bright spots are formed on the road surface, which has a warning effect on the safety of vehicles and pedestrians. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 It is a synthetic gradation curve diagram of the color micro-surfacing concrete in Examples 1 to 5 of the present invention; DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0039] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, a color micro-surfacing concrete proposed according to the present invention, its specific implementation method, characteristics and effects are described in detail as follows. The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.
[0040] In a specific embodiment of the present invention, the sources of various commercially available materials are as follows:
[0041] Material composition Commercial sources gravel Ezhou Changlong Quarry Sand Henan Youji Environmental Protection Technology Co., Ltd. Stained Glass Hubei Jingbo Hailong Glass Products Co., Ltd. cement Huaxin Cement Co., Ltd. Steel slag powder China Baowu Wuhan Iron and Steel Group Co., Ltd. Red Mud Aluminum Corporation of China Limited Emulsified asphalt Shandong Sanju Chemical Technology Co., Ltd. Hexadecyltrimethylammonium chloride Shandong Boxing County Haolong Chemical Co., Ltd. Diisocyanates Zhejiang Lishui Youbang New Materials Co., Ltd.
[0042] Example 1
[0043] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0044] Colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10:20:80:5:1:1:3:1;
[0045] The modified emulsified asphalt is an emulsified asphalt modified by hexadecyltrimethylammonium chloride and diisocyanate, the mass ratio of hexadecyltrimethylammonium chloride is 3‰ of the emulsified asphalt, and the mass ratio of diisocyanate is 2‰ of the emulsified asphalt.
[0046] The mass percentage of the maximum nominal particle size in the colored glass is as follows: 20% of the coarse-grained colored glass is between 2.36mm and 4.75mm, and the Mohs hardness is between 6.3; 80% of the fine-grained colored glass is between 0mm and 2.36mm, and the Mohs hardness is between 5.8. The particle size of the crushed stone is 4.75mm to 9.5mm, and the crushed stone is basalt. The particle size of the sand is 0.075mm to 1.12mm, and the sand is silica sand. The steel slag powder is made by grinding the converter steel slag powder, with a purity of 94% and a particle median diameter of 1.2um. The red mud is steel smelting red mud, which contains 55% iron oxide and a particle median diameter of 0.6mm. The cement is P·O 42.5 silicate cement.
[0047] A method for preparing colored micro-surfacing concrete, comprising:
[0048] (1) Roughening waste glass to obtain colored glass; the roughening process of colored glass includes:
[0049] Put the broken colored glass into the sandblasting room, the sandblasting pressure is 0.5MPa, and the sandblasting speed is 40cm 2 / min, sandblasting time is 5min, and the polishing value of colored glass is 41.
[0050] (2) Preparing modified emulsified asphalt, the preparation method of modified emulsified asphalt comprises:
[0051] S11 Add diisocyanate to water in a ratio of 1:1, adjust the pH to 3 with concentrated hydrochloric acid, and then heat to 76°C while stirring to fully dissolve it;
[0052] S12: asphalt heated to 150°C and diisocyanate are sent to a colloid mill in proportion for emulsification;
[0053] S13, adding cetyl trimethyl ammonium chloride in proportion at the outlet of the emulsified asphalt, and then fully mixing with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt;
[0054] (3) According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder, and red mud were mixed for 40 seconds until uniform, and then water was added and mixed for 35 seconds until it was moistened, and then emulsified asphalt was added and mixed for 35 seconds until it was uniform to obtain colored micro-surfacing concrete.
[0055] Example 2
[0056] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0057] Colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10:25:75:5:2:2:4:1.5;
[0058] The modified emulsified asphalt is an emulsified asphalt modified by hexadecyltrimethylammonium chloride and diisocyanate, the mass ratio of hexadecyltrimethylammonium chloride is 4‰ of the emulsified asphalt, and the mass ratio of diisocyanate is 3‰ of the emulsified asphalt.
[0059] In the colored glass, the mass percentage of the maximum nominal particle size is as follows: 25% of the coarse-grained colored glass of 2.36mm to 4.75mm, with a Mohs hardness of 6.3; 75% of the fine-grained colored glass of 0mm to 2.36mm, with a Mohs hardness of 5.8. The particle size of the crushed stone is 4.75mm to 9.5mm, and the crushed stone is diabase. The particle size of the sand is 0.075mm to 1.12mm, and the sand is silica sand. The steel slag powder is made by grinding the converter steel slag powder, with a purity of 94% and a particle median diameter of 1.2um. The red mud is steel smelting red mud, of which the iron oxide content is 55% and the particle median diameter is 0.6mm. The cement is P·O 42.5 silicate cement.
[0060] A method for preparing colored micro-surfacing concrete, comprising:
[0061] (1) Roughening waste glass to obtain colored glass; the roughening process of colored glass includes:
[0062] Put the broken colored glass into the sandblasting room, the sandblasting pressure is 0.5MPa, and the sandblasting speed is 40cm 2 / min, sandblasting time is 5min, and the polishing value of colored glass is 41.
[0063] (2) Preparing modified emulsified asphalt, the preparation method of modified emulsified asphalt comprises:
[0064] S11 Add diisocyanate to water in a ratio of 1:1, adjust the pH value to 2 with concentrated hydrochloric acid, and then heat to 73°C while stirring to fully dissolve it;
[0065] S12: asphalt heated to 145°C and diisocyanate are sent to a colloid mill in proportion for emulsification;
[0066] S13, adding cetyl trimethyl ammonium chloride in proportion at the outlet of the emulsified asphalt, and then fully mixing with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt;
[0067] (3) According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder, and red mud were mixed for 45 seconds until uniform, and then water was added and mixed for 40 seconds until moistened, and then emulsified asphalt was added and mixed for 40 seconds until uniform to obtain colored micro-surfacing concrete.
[0068] Example 3
[0069] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0070] Colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10:20:80:4:3:2:5:2;
[0071] The modified emulsified asphalt is an emulsified asphalt modified by hexadecyltrimethylammonium chloride and diisocyanate, the mass ratio of hexadecyltrimethylammonium chloride is 4‰ of the emulsified asphalt, and the mass ratio of diisocyanate is 2‰ of the emulsified asphalt.
[0072] In the colored glass, the mass percentage of the maximum nominal particle size is as follows: 30% of the coarse-grained colored glass of 2.36mm to 4.75mm, with a Mohs hardness of 6.3; 70% of the fine-grained colored glass of 0mm to 2.36mm, with a Mohs hardness of 5.8. The particle size of the crushed stone is 4.75mm to 9.5mm, and the crushed stone is limestone. The particle size of the sand is 0.075mm to 1.12mm, and the sand is silica sand. The steel slag powder is made by grinding the converter steel slag powder, with a purity of 94% and a particle median diameter of 1.2um. The red mud is steel smelting red mud, with an iron oxide content of 55% and a particle median diameter of 0.6mm. The cement is P·O 42.5 silicate cement.
[0073] A method for preparing colored micro-surfacing concrete, comprising:
[0074] (1) Roughening waste glass to obtain colored glass; the roughening process of colored glass includes:
[0075] Put the broken colored glass into the sandblasting room, the sandblasting pressure is 0.5MPa, and the sandblasting speed is 40cm 2 / min, sandblasting time is 5min, and the polishing value of colored glass is 41.
[0076] (2) Preparing modified emulsified asphalt, the preparation method of modified emulsified asphalt comprises:
[0077] S11: Add diisocyanate to water in a ratio of 1:1, adjust the pH to 3 with concentrated hydrochloric acid, and then heat to 70°C while stirring to fully dissolve it;
[0078] S12: asphalt heated to 140°C and diisocyanate are sent to a colloid mill in proportion for emulsification;
[0079] S13, adding cetyl trimethyl ammonium chloride in proportion at the outlet of the emulsified asphalt, and then fully mixing with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt;
[0080] (3) According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder, and red mud were mixed for 50 seconds until uniform, and then water was added and mixed for 45 seconds until it was moistened, and then emulsified asphalt was added and mixed for 45 seconds until it was uniform to obtain colored micro-surfacing concrete.
[0081] Example 4
[0082] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0083] Colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10:21:79:4.5:1.5:2:3.5:1;
[0084] The modified emulsified asphalt is an emulsified asphalt modified by hexadecyltrimethylammonium chloride and diisocyanate, the mass ratio of hexadecyltrimethylammonium chloride is 5‰ of the emulsified asphalt, and the mass ratio of diisocyanate is 3‰ of the emulsified asphalt.
[0085] In the colored glass, the mass percentage of the maximum nominal particle size is as follows: 35% of the coarse-grained colored glass of 2.36mm to 4.75mm, with a Mohs hardness of 6.3; 65% of the fine-grained colored glass of 0mm to 2.36mm, with a Mohs hardness of 5.8. The particle size of the crushed stone is 4.75mm to 9.5mm, and the crushed stone is andesite. The particle size of the sand is 0.075mm to 1.12mm, and the sand is silica sand. The steel slag powder is made by grinding the converter steel slag powder, with a purity of 94% and a particle median diameter of 1.2um. The red mud is steel smelting red mud, of which the iron oxide content is 55% and the particle median diameter is 0.6mm. The cement is P·O 42.5 silicate cement.
[0086] A method for preparing colored micro-surfacing concrete, comprising:
[0087] (1) Roughening waste glass to obtain colored glass; the roughening process of colored glass includes:
[0088] Put the broken colored glass into the sandblasting room, the sandblasting pressure is 0.5MPa, and the sandblasting speed is 40cm 2 / min, sandblasting time is 5min, and the polishing value of colored glass is 41.
[0089] (2) Preparing modified emulsified asphalt, the preparation method of modified emulsified asphalt comprises:
[0090] S11: Add diisocyanate to water in a ratio of 1:1, adjust the pH to 3 with concentrated hydrochloric acid, and then heat to 73°C while stirring to fully dissolve it;
[0091] S12: asphalt heated to 145°C and diisocyanate are sent to a colloid mill in proportion for emulsification;
[0092] S13, adding cetyl trimethyl ammonium chloride in proportion at the outlet of the emulsified asphalt, and then fully mixing with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt;
[0093] (3) According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder, and red mud were mixed for 40 seconds until uniform, and then water was added and mixed for 35 seconds until it was moistened, and then emulsified asphalt was added and mixed for 35 seconds until it was uniform to obtain colored micro-surfacing concrete.
[0094] Example 5
[0095] A colored micro-surfacing concrete, the colored micro-surfacing concrete is MS-3 graded asphalt concrete;
[0096] Colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10:27:73:4:2:1:4.5:1.5;
[0097] The modified emulsified asphalt is an emulsified asphalt modified by hexadecyltrimethylammonium chloride and diisocyanate, the mass ratio of hexadecyltrimethylammonium chloride is 2‰ of the emulsified asphalt, and the mass ratio of diisocyanate is 3‰ of the emulsified asphalt.
[0098] The mass percentage of the maximum nominal particle size in the colored glass is as follows: 40% of the coarse-grained colored glass of 2.36mm to 4.75mm, with a Mohs hardness of 6.3; 60% of the fine-grained colored glass of 0mm to 2.36mm, with a Mohs hardness of 5.8. The particle size of the crushed stone is 4.75mm to 9.5mm, and the crushed stone is basalt. The particle size of the sand is 0.075mm to 1.12mm, and the sand is glass sand. The steel slag powder is made by grinding the converter steel slag powder, with a purity of 94% and a particle median diameter of 1.2um. The red mud is steel smelting red mud, with an iron oxide content of 55% and a particle median diameter of 0.6mm. The cement is P·O 42.5 silicate cement.
[0099] A method for preparing colored micro-surfacing concrete, comprising:
[0100] (1) Roughening waste glass to obtain colored glass; the roughening process of colored glass includes:
[0101] Put the broken colored glass into the sandblasting room, the sandblasting pressure is 0.5MPa, and the sandblasting speed is 40cm 2 / min, sandblasting time is 5min, and the polishing value of colored glass is 41.
[0102] (2) Preparing modified emulsified asphalt, the preparation method of modified emulsified asphalt comprises:
[0103] S11 Add diisocyanate to water in a ratio of 1:1, adjust the pH value to 2 with concentrated hydrochloric acid, and then heat to 76°C while stirring to fully dissolve it;
[0104] S12: asphalt heated to 145°C and diisocyanate are sent to a colloid mill in proportion for emulsification;
[0105] S13, adding cetyl trimethyl ammonium chloride in proportion at the outlet of the emulsified asphalt, and then fully mixing with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt;
[0106] (3) According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder, and red mud were mixed for 45 seconds until uniform, and then water was added and mixed for 40 seconds until moistened, and then emulsified asphalt was added and mixed for 40 seconds until uniform to obtain colored micro-surfacing concrete.
[0107] Comparative Example 1
[0108] The only difference between this comparative example and Example 1 is that this comparative example does not contain colored glass and red mud, and specifically, 20% of andesite with a particle size of 2.36mm-4.75mm and 80% of limestone with a particle size of 0mm-2.36mm are used to replace the above-mentioned colored glass, and other details are not repeated here.
[0109] Comparative Example 2
[0110] The only difference between this comparative example and Example 1 is that this comparative example does not contain coarse-grained colored glass and red mud, and specifically uses 20% of basalt with a particle size of 2.36mm-4.75mm to replace the above coarse-grained colored glass, and other details are not repeated here.
[0111] Comparative Example 3
[0112] The only difference between this comparative example and Example 1 is that this comparative example does not contain fine-grained colored glass and red mud, and specifically uses 80% of limestone with a particle size of 0mm-2.36mm to replace the above-mentioned fine-grained colored glass, and other details are not repeated here.
[0113] like Figure 1 It can be seen from the synthetic gradation curve shown that the gradation type of the micro-surfacing pavement material of Examples 1 to 5 is the MS-3 median grade. The specific gradation is shown in Table 1.
[0114] Table 1 Synthetic gradation of MS-3 micro-surfacing pavement materials
[0115] Screen size 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075 Mix ratio Upper limit of gradation 100 90 70 50 34 25 18 15 -- Lower limit of gradation 100 70 45 28 19 12 7 5 -- Median gradation 100.0 80.0 57.5 39.0 26.5 18.5 12.5 10.0 -- Aggregates from 4.75mm to 9.5mm 100 9.2 3.0 2.8 2.7 2.6 2.5 2.4 16% Aggregates 2.37mm-4.75mm 100 92.7 6.6 3.6 2.9 2.8 2.7 2.6 25% Aggregates of 0mm-2.36mm 100 99.8 83.8 66.6 37.9 28.2 19.4 16.7 53.5% Steel slag powder 100 100 100 100 100 99.9 99.7 85.7 4.5% cement 100 100 100 100 100 100 98.1 88.3 1% Synthetic gradation 100 83.5 52.5 42.5 26.9 21.7 16.9 14.7 100.0%
[0116] The micro-surfacing pavement materials of Examples 1 to 5 were prepared into anti-skid and noise-reducing micro-surfacing pavement materials according to the specification of the "Technical Guide for Micro-surfacing and Slurry Seal", and the relevant performance test results are shown in Table 2.
[0117] Table 2 Performance test results of micro-surfacing pavement materials of Examples 1 to 5, Comparative Examples 1 to 3 and MS-3 basalt micro-surfacing pavement materials
[0118]
[0119]
[0120] As shown in Table 2, the mixing time of Examples 1 to 5 is greater than the standard 120s, indicating that the micro-surfacing concrete has good construction performance. Parameters such as 1h wet wheel wear and rutting deformation rate are slightly higher than those of ordinary basalt micro-surfacing pavement materials, but they all meet the requirements of the "Technical Guidelines for Micro-surfacing and Slurry Seal" and meet basic road performance.
[0121] Compared with the basalt micro-surfacing pavement material, Examples 1 to 5 have higher BPN values, indicating that the skid resistance of the colored micro-surfacing pavement of Examples 1 to 5 is better than that of the basalt micro-surfacing pavement. The BPN value of Comparative Example 1 is significantly lower than that of Comparative Example 2 and Comparative Example 3, indicating that colored glass can significantly improve the skid resistance of the material. Compared with the basalt micro-surfacing pavement material, Examples 1 to 5 have higher reflection coefficient values, indicating that the nighttime visualization effect of the micro-surfacing concrete of Examples 1 to 5 is better than that of the basalt micro-surfacing pavement material. The reflection coefficient value of Comparative Example 1 is significantly lower than that of Comparative Example 2 and Comparative Example 3, indicating that colored glass can significantly improve the nighttime visibility of the micro-surfacing pavement.
[0122] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A colored micro-surfacing concrete, characterized in that: The colored micro-surfacing concrete is MS-3 graded asphalt concrete; The colored micro-surfacing concrete is prepared by mixing crushed stone, sand, colored glass, cement, steel slag powder, red mud, modified emulsified asphalt and water in a mass ratio of 10-20:20-30:70-80:3-5:1-3:1-2:3-5:1-2; The modified emulsified asphalt is an emulsified asphalt modified by a cationic surfactant and a vulcanized crosslinking agent, wherein the mass ratio of the cationic surfactant is 2‰ to 5‰ of the emulsified asphalt, and the mass ratio of the vulcanized crosslinking agent is 2‰ to 3‰ of the emulsified asphalt.
2. The colored micro-surfacing concrete according to claim 1, characterized in that: In the colored glass, the mass percentage of the maximum nominal particle size is as follows: 2.36mm~4.75mm coarse-grained colored glass, 20%~40%; 0mm~2.36mm fine particle size colored glass, 60%~80%.
3. The colored micro-surfacing concrete according to claim 1, characterized in that: The colored glass is obtained by roughening waste glass; the Mohs hardness of the colored glass is between 5.4 and 6.5; the roughening process of the colored glass includes: Place the broken colored glass in the sandblasting room, the sandblasting pressure is 0.2MPa~0.6MPa, and the sandblasting speed is 30cm 2 / min~50cm 2 / min, sandblasting time is 4min~6min, and the polishing value of colored glass is 36~42.
4. The colored micro-surfacing concrete according to claim 1, characterized in that: The particle size of the crushed stone is 4.75 mm to 9.5 mm, and the crushed stone includes any one or more combinations of diabase, andesite, limestone, and basalt.
5. The colored micro-surfacing concrete according to claim 1, characterized in that: The particle size of the sand particles is 0.075 mm to 1.12 mm, and the sand particles include any one or more combinations of silica sand, glass sand, and corundum.
6. The colored micro-surfacing concrete according to claim 1, characterized in that: The steel slag powder is produced by grinding converter steel slag, with a purity of 90% to 100% and a particle median diameter of 0.8um to 12um.
7. The colored micro-surfacing concrete according to claim 1, characterized in that: The red mud is steel smelting red mud, wherein the iron oxide content is 35% to 65% and the particle median diameter is 0.075 mm to 1.12 mm.
8. The colored micro-surfacing concrete according to claim 1, characterized in that: The preparation method of the modified emulsified asphalt comprises: S11 Add the vulcanized crosslinking agent to water at a ratio of 1:1, adjust the pH value to 2-3 with concentrated hydrochloric acid, and then heat to 70-76°C while stirring to fully dissolve it; S12 sends the asphalt heated to 140-150°C and the vulcanized cross-linking agent into the colloid mill for emulsification in proportion; S13 adds a cationic surfactant in proportion at the outlet of the emulsified asphalt, and then fully mixes it with a stirrer in the emulsified asphalt storage to obtain modified emulsified asphalt.
9. The colored micro-surfacing concrete according to claim 8, characterized in that: The cationic surfactant is hexadecyltrimethylammonium chloride; and the vulcanization crosslinking agent is diisocyanate.
10. The method for preparing colored micro-surfacing concrete according to claim 1, characterized in that: include: According to the proportion of each component, crushed stone, sand, colored glass, cement, steel slag powder and red mud are mixed, then water is added to moisten, and then modified emulsified asphalt is added to mix to obtain the colored micro-surfacing concrete.