High-stability permanent magnetic ferrite material and preparation method thereof

By employing novel ball milling processes, element doping, optimized sintering processes, and heat treatment technologies, the stability and cost issues of permanent magnet ferrite materials in traditional processes have been resolved, resulting in the preparation of permanent magnet ferrite materials with high stability and high magnetic properties.

CN118930242AInactive Publication Date: 2024-11-12ANHUI ONE MAGNET ELECTRONIC CO LTD

Patent Information

Application Number
CN202411073524.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare permanent magnet ferrite materials that are both low-cost and highly stable. The addition of heavy rare earth elements in traditional production processes leads to decreased material stability and increased costs.

Method used

By employing novel ball milling technology, element doping technology, optimized sintering process and heat treatment technology, combined with refined microstructure control, highly stable permanent magnet ferrite materials are prepared.

Benefits of technology

It significantly improves the magnetic properties and stability of permanent magnet ferrites, reduces production costs, and achieves high density and excellent performance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930242A_ABST
    Figure CN118930242A_ABST
Patent Text Reader

Abstract

The invention discloses a high-stability permanent magnetic ferrite material and a preparation method thereof, and belongs to the technical field of rare earth magnetic materials. The method comprises the following steps: carrying out primary ball-milling on preparation raw materials to obtain slurry, drying, pre-sintering, crushing and sieving to obtain pre-sintered material particles, adding a rare earth oxide additive and water, carrying out secondary ball-milling to obtain secondary ball-milled slurry, applying a magnetic field to the secondary ball-milled slurry for orientation, carrying out compression molding to obtain a green body, and sintering to obtain the permanent magnetic ferrite, and finally, solid solution treatment, magnetic field heat treatment and tempering heat treatment are conducted. By adopting a novel element doping technology, a microstructure fine control technology, an efficient ball milling technology, an optimized sintering technology and an advanced heat treatment technology, the comprehensive magnetic performance and the stability of the permanent magnetic ferrite are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth permanent magnetic materials, and in particular relates to a highly stable permanent magnetic ferrite material and a preparation method thereof. Background Art

[0002] Permanent ferrite, also known as hard ferrite, is a new type of non-metallic magnetic material. It only needs to provide magnetizing energy once to generate a stable magnetic field, thereby continuously providing magnetic energy to the outside. The current era is the electronic era. Without permanent ferrite, there would be no electronic industry. As a basic functional material of the electronic industry, permanent ferrite has penetrated into all areas of human production and life. It has been widely used in automobiles, computers, medical instruments, etc., and it is an important aspect of energy development. Whether from the perspective of resources or applications, the development prospects of permanent ferrite are very broad. In addition, relevant national policy documents also point out the development direction of rare earth permanent magnetic materials, requiring the reduction of rare earth consumption while improving comprehensive magnetic properties and promoting the efficient use of rare earths. With the strengthening of national control over the rare earth industry, the price of raw materials has continued to rise. Therefore, a large amount of heavy rare earth elements are added in the traditional production process, resulting in a decrease in the stability of permanent ferrite and a sharp increase in costs. At present, my country's production of permanent ferrite mainly uses iron red and iron scale. Iron red is expensive as a production raw material, and iron scale is a by-product of steel rolling mills and is recycled, but the iron scale composition is complex and unstable. Therefore, finding cheap alternative raw materials for the production of permanent magnet ferrites, reducing the production cost of permanent magnet ferrites, and improving the stability of ferrites are currently urgent issues in the production of permanent magnet ferrites.

[0003] It is impossible to prepare highly stable permanent magnet ferrite materials using traditional production methods, so it is necessary to develop a highly stable permanent magnet ferrite material and a preparation method thereof to reduce production costs and improve stability. Summary of the invention

[0004] The object of the present invention is to provide a highly stable permanent magnetic ferrite material and a preparation method thereof, so as to solve the problem that it is difficult to prepare a permanent magnetic ferrite material with low cost and high stability in the prior art.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] S1. Using a new ball milling process, ferric oxide, silicon oxide, industrial strontium carbonate and water are ball milled once;

[0007] S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles;

[0008] S3. The pre-sintered material particles and rare earth oxide additives, water mixed secondary ball milling, to obtain a secondary ball milling slurry;

[0009] S4. Orienting the secondary ball-milled slurry with a magnetic field and pressing it to obtain a green embryo;

[0010] S5. The green embryo is dried by optimizing the sintering process, and then the temperature is gradually increased to 1080-1120°C to obtain the permanent ferrite;

[0011] S6. Perform solid solution treatment, magnetic field heat treatment and tempering heat treatment on the permanent ferrite.

[0012] Furthermore, in S1, the volume ratio of ball milling medium: preparation raw material: water is 90-92%: 4-5%: 4-5%, and the ball milling time is 3-3.5h.

[0013] Furthermore, the pre-burning temperature in S2 is 1200-1280° C., the heating time is 6-6.5 h, and the heat preservation time is 0.5-1 h.

[0014] Furthermore, the mesh size of the crushed and screened sieve in S2 is 100 meshes.

[0015] Furthermore, the rare earth oxide additives in S3 are cobalt trioxide and lanthanum oxide.

[0016] Furthermore, the particle size of the secondary ball-milled slurry in S3 is 0.8-0.9 μm.

[0017] Furthermore, in S3, the volume ratio of ball milling medium: pre-sintered material particles: water: rare earth oxide additive is 90-92%: 4-5%: 3-4%: 0.2-1%, and the ball milling time is 3-3.5h.

[0018] Furthermore, in S5, the gradient heating starts from room temperature, is heated to 500°C at 25°C / min, is kept warm for 1 hour, and then is heated from 500°C at 25°C / min to 1100°C, and is kept warm for 2 hours.

[0019] Furthermore, the solution treatment temperature in S6 is 1200-1280° C., and cold water quenching is adopted.

[0020] Furthermore, the magnetic field heat treatment in S6 is carried out in a heat treatment furnace with a micro-field strength greater than 200 kA / m, and isothermally treated at 640-650° C. for 1-2 hours.

[0021] Furthermore, the tempering heat treatment in S6 is performed as a stepped multi-stage tempering, and the step temperatures and the holding times thereof are set to 620° C., 1 h; 610° C., 1 h; 590° C., 2 h; 570° C., 3 h; and 540° C., 5 h.

[0022] A highly stable permanent magnetic ferrite material is prepared by the above preparation method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention adopts a new element doping technology, which optimizes the material composition of permanent ferrite by introducing new elements for doping, and significantly improves its magnetic properties and stability. This element doping technology can effectively regulate the electronic structure and magnetic domain structure of the material, thereby achieving a breakthrough in magnetic properties.

[0025] 2. The present invention adopts a microstructure fine control process, and realizes fine control of the microstructure of permanent ferrite through advanced preparation process and heat treatment technology. By adjusting the grain size, shape and orientation, the magnetic domain arrangement and magnetic flux path of the magnet are optimized, and the magnetic properties of the magnet are further improved.

[0026] 3. The present invention adopts high-efficiency ball milling technology: develops a new ball milling process, improves ball milling efficiency, reduces energy consumption, and ensures the uniformity and fineness of the magnet components, providing a good foundation for the subsequent sintering process.

[0027] 4. The present invention adopts an optimized sintering process: by improving parameters such as temperature, atmosphere and time during the sintering process, high density and excellent performance of the magnet are achieved.

[0028] 5. The present invention adopts advanced heat treatment technology, including solution treatment, magnetic field heat treatment, and tempering heat treatment, to further eliminate stress and defects inside the magnet and improve the stability and reliability of the magnet. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a flow chart of a highly stable permanent ferrite material and a preparation method thereof according to an embodiment of the present application. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] See also Figure 1 , a highly stable permanent magnetic ferrite material and a preparation method thereof, comprising the following steps:

[0033] S1. Using a new ball milling process, ferric oxide, silicon oxide, industrial strontium carbonate and water are ball milled once;

[0034] S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles;

[0035] S3. The pre-sintered material particles, rare earth oxide additives and water are mixed and subjected to secondary ball milling to obtain a secondary ball milling slurry;

[0036] S4. Orienting the secondary ball-milled slurry with a magnetic field and pressing it to obtain a green embryo;

[0037] S5. The green embryo is dried by optimizing the sintering process, and then the temperature is gradually increased to 1080-1120°C to obtain the permanent ferrite;

[0038] S6. Perform solid solution treatment, magnetic field heat treatment and tempering heat treatment on the permanent ferrite.

[0039] Comparative Example 1:

[0040] A highly stable permanent magnetic ferrite material and a preparation method thereof are the same as those in Example 1, except that in S1, a conventional ball milling process is used to ball mill ferric oxide, silicon oxide, industrial strontium carbonate and water, and other components and parameters remain unchanged.

[0041] Comparative Example 2:

[0042] A highly stable permanent magnetic ferrite material and a preparation method thereof are the same as those in Example 1, except that the raw material in S1 is not doped with industrial strontium carbonate, and the other components and parameters remain unchanged.

[0043] Comparative Example 3:

[0044] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as those in Example 1, except that a conventional sintering process is used in S5, and other components and parameters remain unchanged.

[0045] Comparative Example 4:

[0046] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as those in Example 1, except that no solid solution treatment is performed in S6, and other components and parameters remain unchanged.

[0047] Comparative Example 5:

[0048] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as those in Example 1, except that no magnetic field heat treatment is performed in S6, and other components and parameters remain unchanged.

[0049] Comparative Example 6:

[0050] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as those in Example 1, except that no tempering heat treatment is performed in S6, and other components and parameters remain unchanged.

[0051] Comparative Example 7:

[0052] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as in Example 1, except that gradient temperature rise sintering is not adopted, and the temperature is directly raised from room temperature to 1100°C at a heating rate of 10°C / min, kept at that temperature for 2h, and finally cooled to room temperature with the furnace, and the other components and parameters remain unchanged.

[0053] Comparative Example 8:

[0054] A highly stable permanent magnet ferrite material and a preparation method thereof are the same as those in Example 1, except that S1 adopts a traditional ball milling process, S1 is not doped with industrial strontium carbonate, S5 adopts a traditional sintering process, S6 does not perform heat treatment, and the other components and parameters remain unchanged.

[0055] The magnet properties of the above different embodiments and comparative examples were tested at 25° C. The test results are shown in Table 1.

[0056] Table 1

[0057]

[0058] It can be seen from Table 1 that the use of new element doping technology, efficient ball milling process, microstructure fine control process and optimized sintering process can prepare permanent magnet ferrite with remanence higher than 12.8KGs, intrinsic coercive force greater than 35KOe, and maximum magnetic energy product higher than 35BH. It can be seen from Example 1 and Comparative Example 1 that the use of new ball milling process can greatly improve the squareness of the magnet, while ensuring the uniformity and fineness of the magnet components, and comprehensively improve the magnetic properties. It can be seen from Example 1 and Comparative Example 3 that the use of optimized sintering process can improve the high density and excellent performance of the magnet. It can be seen from Example 1 and Comparative Examples 4-6 that heat treatment of sintered permanent magnet ferrite can effectively improve the comprehensive magnetic properties. It can be seen from Example 1 and Comparative Example 7 that the preparation method using gradient heating can effectively improve the remanence and maximum magnetic energy product of the magnet. It can be seen from Example 1 and Comparative Example 8 that the optimization of each process in the preparation process of permanent magnet ferrite has a significant effect, which greatly improves the comprehensive magnetic properties of permanent magnet ferrite.

[0059] The magnet properties of Example 1 and Comparative Example 2 were tested at 35°C. The test results are shown in Table 2.

[0060] Table 2

[0061]

[0062] The magnet properties of Example 1 and Comparative Example 2 were tested at 45°C. The test results are shown in Table 3.

[0063] Table 3

[0064]

[0065] The magnet properties of Example 1 and Comparative Example 2 were tested at 55° C. The test results are shown in Table 4.

[0066] Table 4

[0067]

[0068] As can be seen from Tables 1-4, by introducing new elements for doping, the material composition of permanent ferrite is optimized, and its magnetic properties and stability are significantly improved. This element doping technology can effectively regulate the electronic structure and magnetic domain structure of the material, thereby achieving a breakthrough in magnetic properties.

[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A highly stable permanent ferrite material and a preparation method thereof, It is characterized in that The following steps are involved: S1. Using a new ball milling process, ferric oxide, silicon oxide, industrial strontium carbonate and water are ball milled once; S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles; S3. The pre-sintered material particles and rare earth oxide additives, water mixed secondary ball milling, to obtain a secondary ball milling slurry; S4. Orienting the secondary ball-milled slurry with a magnetic field and pressing it to obtain a green embryo; S5. The green embryo is dried by optimizing the sintering process, and then the temperature is gradually increased to 1080-1120°C to obtain the permanent ferrite; S6. Perform solid solution treatment, magnetic field heat treatment and tempering heat treatment on the permanent ferrite.

2. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that In the S1, the volume ratio of ball milling medium: preparation raw material: water is 90-92%: 4-5%: 4-5%, and the ball milling time is 3-3.5h.

3. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The pre-burning temperature in S2 is 1200-1280° C., the heating time is 6-6.5 hours, and the heat preservation time is 0.5-1 hour.

4. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The mesh number of the crushed and sieved sieve in S2 is 100 meshes.

5. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The rare earth oxide additives in S3 are cobalt trioxide and lanthanum oxide.

6. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The particle size of the secondary ball-milled slurry in S3 is 0.8-0.9 μm.

7. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The volume proportions of ball milling medium: pre-sintered material particles: water: rare earth oxide additive in S3 are 90-92%: 4-5%: 3-4%: 0.2-1%, and the ball milling time is 3-3.5h.

8. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that In the S5, the temperature is gradually increased from room temperature to 500°C at a rate of 25°C / min, and kept at that temperature for 1 hour. Then, the temperature is gradually increased from 500°C to 1100°C at a rate of 25°C / min, and kept at that temperature for 2 hours.

9. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, It is characterized in that The solution treatment temperature of S6 is 1200-1280°C, and cold water quenching is adopted; the magnetic field heat treatment of S6 is carried out in a heat treatment furnace with a micro-field strength greater than 200kA / m, and isothermal treatment is performed at 640-650°C for 1-2h; the tempering heat treatment of S6 is a step-by-step multi-step tempering, and the step temperature and its holding time are set to 620°C, 1h; 610°C, 1h; 590°C, 2h; 570°C, 3h; 540°C, 5h.

10. A highly stable permanent ferrite material, It is characterized in that Prepared by the production process described in any one of claims 1 to 11.

Citation Information

Patent Citations

  • Permanent magnetic ferrite preparation method

    CN103232232A

  • Sm2Co17 type sintered magnet with low temperature coefficient and preparation method thereof

    CN111091943A

  • Samarium cobalt rare earth permanent magnet and preparation method thereof

    CN115547603A

  • High-squareness samarium-cobalt permanent magnet material and preparation method thereof

    CN118098739A

  • Sintered ferrite preparation process and sintered ferrite magnet

    CN118213180A

Cited By

  • Permanent magnetic ferrite with high thermal stability as well as preparation method and application of permanent magnetic ferrite

    CN121494524A