Zinc oxide target material and preparation method thereof
Through the multi-stage hot press sintering method, the sintering temperature of zinc oxide targets is reduced, the formation of zinc aluminate is reduced, and the conductivity and bending strength are improved, which solves the problems of reduced conductivity and cost increase caused by high-temperature sintering in the prior art.
Patent Information
- Application Number
- CN202411295101.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-15
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing zinc oxide target preparation methods, high temperature sintering is easy to generate zinc aluminate, which affects the conductivity of the target material, and high sintering temperature leads to an increase in cost.
Multi-stage hot press sintering method is adopted, the first hot press sintering temperature is 400-600℃, the pressure is 2-4MPa, the second hot press sintering temperature is 1200-1300℃, and the pressure is 20-30MPa, which is reduced by spray granulation and vacuum environment. Crystal growth temperature reduces zinc aluminate formation.
It effectively improves the density and bending strength of zinc oxide targets, enhances conductivity, reduces sintering temperature, extends the service life of the target, and reduces the conductivity reduction.
Smart Images

Figure BDA0005045719110000071 
Figure BDA0005045719110000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of target material preparation, and in particular to a zinc oxide target material and a preparation method thereof. Background Art
[0002] In recent years, with the introduction and realization of the concepts of intelligence and informationization, more and more electronic devices have appeared in people's lives: display screens, various sensors, solar cells, etc., and these devices, especially solar cells, require TCO films (transparent conductive films) as electrode layers or conductive layers. Zinc oxide (ZnO) is a material with good visible light transmittance, high infrared reflectivity, wide band gap, and excellent conductivity. It has the advantages of wide material sources, good doping, and low cost. It is widely used in the preparation of TCO films.
[0003] Generally, there are many methods for preparing TCO thin films, such as physical vapor deposition, chemical vapor deposition, evaporation, molecular beam epitaxy, magnetron sputtering, etc. Among them, magnetron sputtering using ZnO-based targets is more suitable for preparing TCO thin films in large quantities. At the same time, other film-making methods also require ZnO-based targets. The performance of the target material largely determines the performance of the prepared TCO thin film. The composition, density, resistivity, grain size and other optoelectronic physical properties of the target material will comprehensively determine the actual application effect of the TCO thin film.
[0004] Chinese patent application 202310656739.7 discloses a gallium-aluminum-doped zinc oxide target material and its preparation method and application, wherein the preparation steps include: placing a main oxide mixed powder, a modifier, a grain refiner, a dispersant, a binder, a wetting agent and water in a stirring barrel and stirring and mixing them evenly to form a mixed slurry; passing the mixed slurry into a grinder for sufficient grinding; passing the ground mixed slurry into a spray granulation dryer for spray drying and granulation to obtain gallium-aluminum-doped zinc oxide powder; first pressing the obtained powder under low pressure and then under high pressure to obtain a target blank; finally placing the blank in a sintering furnace for two-stage heat preservation sintering;
[0005] The target material prepared by this scheme has the characteristics of low cost and significantly improved electrical and optical properties of the target material;
[0006] However, further observation of the scheme shows that its sintering mainly includes the following stages:
[0007] Debinding is carried out at 500-600℃, and the holding time is 2-4h;
[0008] Low temperature sintering is carried out at 700-800℃, and the holding time is 4-8h;
[0009] High temperature sintering is carried out at 1200-1400℃, and the holding time is 12-24h;
[0010] The purpose of sintering at 500-600℃ is mainly to remove binder, because some dispersants, binders, etc. are added to the raw materials;
[0011] Therefore, 700-800°C is the first sintering temperature. It can be seen that the first sintering temperature of this scheme is slightly higher, and the insulation time is slightly longer. Aluminum oxide and zinc oxide are easy to generate zinc aluminate at high temperature. At the same time, with the generation of zinc aluminate, the conductivity of the target material may be adversely affected to a certain extent.
[0012] Chinese patent application 201310334546.6 discloses a method for preparing aluminum-gallium co-doped zinc oxide nanopowder and a high-density high-conductivity sputtering coating target thereof, wherein the preparation steps of the scheme are: 1. dissolving high-purity metal into transparent aluminum nitrate, zinc nitrate and gallium nitrate solutions;
[0013] 2. Ingredients: Divide the three transparent solutions into containers according to the proportion;
[0014] 3. Chemical precipitation: The three transparent solutions are treated in proportion and in a prescribed process by homogeneous coprecipitation method to obtain aluminum-gallium co-doped zinc oxide nanopowder;
[0015] 4. Cleaning: Rinse the mixed precipitate with deionized water and stir thoroughly until there are no other ions;
[0016] 5. Calcination: Place the nano powder in a high temperature furnace for calcination to obtain aluminum-gallium co-doped zinc oxide nano powder;
[0017] 6. Granulation: adding aluminum-gallium co-doped nano zinc oxide powder to a binder and drying to obtain aluminum-gallium co-doped nano zinc oxide powder before molding;
[0018] 7. Molding: Press the aluminum-gallium co-doped zinc oxide pre-molding powder into a primary embryo;
[0019] 8. Sintering: Place the embryo into a high temperature furnace for normal pressure sintering or gas pressure sintering;
[0020] Further observation of step 5 of the scheme shows that the calcination temperature in the first calcination process of step 5 is 850°C and the calcination time is 8 hours;
[0021] Although this scheme improves the density and conductivity of the target material by doping with gallium, there is still room for further reduction of the primary sintering temperature of this scheme.
[0022] The problem that this proposal needs to solve: How to propose a method for preparing zinc oxide target material by low-temperature sintering. Summary of the invention
[0023] The purpose of the present invention is to provide a method for preparing a zinc oxide target under low-temperature sintering conditions. Due to the lower sintering temperature, the generation of zinc aluminate that has an adverse effect on the electrical conductivity of the target can be suppressed as much as possible, thereby improving the electrical conductivity of the target.
[0024] To achieve the above object, the present application discloses a method for preparing a zinc oxide target, comprising the following steps:
[0025] Step 1: Mix zinc oxide powder, aluminum oxide powder and gallium oxide powder, and spray granulate to obtain powder;
[0026] Step 2: hot pressing and sintering the powder obtained in step 1 once, hot pressing and sintering twice, and then cooling and reducing pressure to obtain a zinc oxide target;
[0027] During the primary hot pressing sintering process, the temperature is 400-600°C and the pressure is 2-4MPa;
[0028] During the secondary hot pressing sintering process, the temperature is 1200-1300°C and the pressure is 20-30MPa.
[0029] By hot pressing sintering, the temperature required for the crystal growth of the target material can be effectively reduced, thereby reducing the sintering temperature of the zinc oxide target material, thereby reducing the formation of zinc aluminate and reducing the reduction in electrical conductivity.
[0030] Preferably, the mass ratio of zinc oxide powder, aluminum oxide powder and gallium oxide powder is 96-98.5:1-3:0.5-1.
[0031] Preferably, in step 1, the powder obtained by spray granulation includes powder 1 and powder 2, the average particle size of powder 1 is 25 to 60 μm, and the average particle size of powder 2 is 60 to 90 μm and does not include 60 μm.
[0032] Preferably, step 1 is specifically:
[0033] Firstly, zinc oxide powder and aluminum oxide powder are mixed and spray granulated to obtain powder 1;
[0034] The zinc oxide powder and the gallium oxide powder are mixed and spray granulated to obtain a second powder;
[0035] In the powder 1 and the powder 2, the mass ratio of zinc oxide is 1:4-5.
[0036] Preferably, step 2 is performed in a vacuum environment, and the vacuum degree of the vacuum environment is not higher than 10Pa.
[0037] Preferably, the primary hot pressing sintering is specifically as follows: placing the powder obtained in step 1 in a vacuum environment, first heating the temperature to 400-600° C. at a heating rate of 0.5-1° C. / min, while increasing the pressure to 2-4 MPa, and maintaining the temperature and pressure for 1.5-3 hours;
[0038] The secondary hot pressing sintering is specifically as follows: the material that has completed the primary sintering is heated to 1200-1300°C at a heating rate of 1-2°C / min, and the pressure is increased to 20-30MPa, and the temperature and pressure are maintained for 4-6 hours.
[0039] In addition, the present application also discloses a zinc oxide target material, which is prepared by the above-mentioned method for preparing the zinc oxide target material.
[0040] Preferably, the flexural strength of the zinc oxide target is not less than 140 MPa, and the electrical conductivity is not less than 500 s / cm.
[0041] The beneficial effects of the present invention are:
[0042] The present invention provides a method for preparing a zinc oxide target material. Due to multi-stage hot pressing and sintering, the density of the target material can be effectively improved, thereby improving the bending strength of the target material, making it difficult for the target material to crack during sputtering, and improving the service life of the target material.
[0043] At the same time, the present application chooses to introduce gallium oxide and aluminum oxide into the zinc oxide target material to effectively increase the conductivity of the zinc oxide target material;
[0044] Furthermore, the present application can effectively reduce the temperature required for crystal growth of the target material through hot pressing sintering, thereby reducing the sintering temperature of the zinc oxide target material, thereby reducing the generation of zinc aluminate and reducing the reduction in electrical conductivity. DETAILED DESCRIPTION
[0045] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0046] Example 1
[0047] Step 1: zinc oxide powder, aluminum oxide powder and gallium oxide powder are mixed in a mass ratio of 97.2:2:0.8, and spray granulated to obtain a powder with an average particle size of 60 μm;
[0048] Step 2: The mixture obtained in step 1 is loaded into a mold, and then placed in a vacuum hot pressing furnace, and the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 7 Pa, the temperature is first increased to 500°C at a heating rate of 0.8°C / min, and the pressure is increased to 3MPa, and the temperature and pressure are maintained for 2 hours;
[0049] The material that has completed the primary hot pressing sintering is heated to 1250°C at a heating rate of 1.5°C / min, and the pressure is increased to 25MPa, and the temperature and pressure are maintained for 5 hours.
[0050] After step 2 is completed, the furnace door is opened and the mold is removed to obtain a zinc oxide target with a bending strength of 154.4 MPa and an electrical conductivity of 519.1 s / cm.
[0051] Example 2
[0052] Step 1: Mix zinc oxide powder, aluminum oxide powder and gallium oxide powder in a mass ratio of 96:3:1, spray granulate, and obtain a powder with an average particle size of 60 μm;
[0053] Step 2: The mixture obtained in step 1 is loaded into a mold, and then placed in a vacuum hot pressing furnace, and the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 9 Pa, the temperature is first increased to 600°C at a heating rate of 1°C / min, and the pressure is increased to 2MPa, and the temperature and pressure are maintained for 1.5 hours;
[0054] The material that has completed the primary hot pressing sintering is heated to 1300°C at a heating rate of 2°C / min, and the pressure is increased to 20MPa, and the temperature and pressure are maintained for 6 hours.
[0055] After step 2 is completed, the furnace door is opened and the mold is removed to obtain a zinc oxide target with a bending strength of 144.7 MPa and an electrical conductivity of 505.1 s / cm.
[0056] Example 3
[0057] Step 1: zinc oxide powder, aluminum oxide powder and gallium oxide powder are mixed in a mass ratio of 98.5:1:0.5, and spray granulated to obtain a powder with an average particle size of 60 μm;
[0058] Step 2: The mixture obtained in step 1 is loaded into a mold, and then placed in a vacuum hot pressing furnace, and the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 8 Pa, the temperature is first increased to 400°C at a heating rate of 0.5°C / min, and the pressure is increased to 4MPa, and the temperature and pressure are maintained for 3 hours;
[0059] The material that has completed the primary hot pressing sintering is heated to 1200°C at a heating rate of 1°C / min, and the pressure is increased to 30MPa, and the temperature and pressure are maintained for 4 hours.
[0060] After step 2 is completed, the furnace door is opened and the mold is removed to obtain a zinc oxide target with a bending strength of 147.5 MPa and an electrical conductivity of 507.6 s / cm.
[0061] Example 4
[0062] The method is basically the same as Example 1, except that step 1 is specifically as follows:
[0063] Zinc oxide powder, aluminum oxide powder, and gallium oxide powder were mixed in a mass ratio of 97.2:2:0.8, and spray granulated to obtain powder 1 with an average particle size of 52 μm and powder 2 with an average particle size of 62 μm, and the mass ratio of powder 1 to powder 2 was 21.44:78.56;
[0064] Finally, a zinc oxide target with a flexural strength of 158.6 MPa and an electrical conductivity of 519.4 s / cm was obtained.
[0065] Example 5
[0066] The method is basically the same as Example 1, except that step 1 is specifically as follows:
[0067] Firstly, zinc oxide powder and aluminum oxide powder are mixed and spray granulated to obtain powder 1; and then the powder and aluminum oxide powder are mixed in a mass ratio of 19.44:2 and spray granulated to obtain powder 1 with a particle size of 52 μm;
[0068] Then, zinc oxide powder and gallium oxide powder are mixed in a mass ratio of 77.76:0.8, and spray granulated to obtain powder 2 with a particle size of 62 μm, and the mass ratio of powder 1 to powder 2 is 21.44:78.56;
[0069] Finally, a zinc oxide target with a flexural strength of 159.2 MPa and an electrical conductivity of 526.4 s / cm was obtained.
[0070] Example 6
[0071] The method is basically the same as Example 1, except that step 1 is specifically as follows:
[0072] First, zinc oxide powder and aluminum oxide powder are mixed and spray granulated to obtain powder 1; and then the mixture is mixed in a mass ratio of 16.2:2 and spray granulated to obtain powder 1 with a particle size of 48 μm;
[0073] Then, zinc oxide powder and gallium oxide powder are mixed in a mass ratio of 81:0.8, and spray granulated to obtain powder 2 with a particle size of 62.7 μm, and the mass ratio of powder 1 to powder 2 is 18.2:81.8;
[0074] Finally, a zinc oxide target with a flexural strength of 157.9 MPa and an electrical conductivity of 520.4 s / cm was obtained.
[0075] Example 7
[0076] The method is basically the same as Example 1, except that step 1 is specifically as follows:
[0077] First, zinc oxide powder and aluminum oxide powder were mixed in a mass ratio of 17.7:2, and spray granulated to obtain a powder with a particle size of 49.3 μm.
[0078] Then, zinc oxide powder and gallium oxide powder were mixed in a mass ratio of 79.5:0.8, and spray granulated to obtain powder 2 with a particle size of 62.6 μm, and the mass ratio of powder 1 to powder 2 was 19.7:80.3;
[0079] Finally, a zinc oxide target with a flexural strength of 158.1 MPa and an electrical conductivity of 519.8 s / cm was obtained.
[0080] Comparative Example 1
[0081] The method is basically the same as Example 1, except that step 2 is specifically as follows:
[0082] The mixture obtained in step 1 is loaded into a mold, and then placed in a vacuum hot pressing furnace, and the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 7 Pa, the temperature is first increased to 700°C at a heating rate of 0.8°C / min, and the pressure is increased to 3MPa, and the temperature and pressure are maintained for 2 hours;
[0083] The material that has completed the primary hot pressing sintering is heated to 1250°C at a heating rate of 1.5°C / min, and the pressure is increased to 25MPa, and the temperature and pressure are maintained for 5 hours.
[0084] After step 2 is completed, the furnace door is opened and the mold is removed to obtain a zinc oxide target with a bending strength of 142.2 MPa and an electrical conductivity of 378.3 S / cm.
[0085] Comparative Example 2
[0086] The method is basically the same as Example 1, except that step 2 is specifically as follows:
[0087] The mixture obtained in step 1 is loaded into a mold, and then placed in a vacuum hot pressing furnace, and the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 7 Pa, the temperature is first increased to 500°C at a heating rate of 0.8°C / min, and kept warm for 2h;
[0088] The material that has completed the first hot pressing sintering is heated to 1250°C at a heating rate of 1.5°C / min and kept at this temperature for 5 hours.
[0089] After step 2 is completed, the furnace door is opened and the mold is removed to obtain a zinc oxide target with a bending strength of 96.8 MPa and an electrical conductivity of 328.6 s / cm.
[0090] Performance Test:
[0091] The bending strength and electrical conductivity of the target material prepared by the embodiment and the comparative example were tested by the three-point bending method and the four-probe method, respectively. The results are shown in Table 1:
[0092] Table 1
[0093]
[0094]
[0095] Result analysis:
[0096] 1. It can be seen from Examples 1-3 that when some process parameters in the target material preparation process are slightly adjusted, the bending strength and conductivity of Examples 1-3 fluctuate to a certain extent, but the overall fluctuation is small;
[0097] 2. It can be seen from Examples 1 and 4 that when the powder is made into powder 1 and powder 2 with different average particle sizes, although the total average particle sizes of powder 1 and powder 2 in Example 4 are close to that in Example 1, the flexural strength of Example 4 is still improved to a certain extent relative to that of Example 1. It can be seen that the combined use of powders of various particle sizes can improve the density of the target material and thus improve the flexural strength;
[0098] Further observation of Examples 5-7 shows that when zinc oxide and aluminum oxide are used to prepare powder 1, zinc oxide and gallium oxide are used to prepare powder 2, and the mass ratio of powder 1 to the mass ratio of zinc oxide in powder 2 is 1:4-5, the conductivity and bending strength of the obtained zinc oxide target are improved to varying degrees relative to Example 1;
[0099] The reason for this phenomenon is that, on the one hand, the density of the target material is improved by the coordination between powders of different particle sizes. On the other hand, this treatment makes the small-particle powder 1 a mixture of zinc oxide and aluminum oxide; the large-particle powder 2 a mixture of zinc oxide and gallium oxide. At the same time, because the powder 1 not only has a smaller particle size, but also has a smaller mass proportion, during the mixing process, the small-particle powder 1 composed of a mixture of zinc oxide and aluminum oxide is more filled in the gaps of the powder 2, so that the heating of the powder 1 is relatively more uniform, thereby inhibiting the formation of zinc aluminate, thereby improving the conductivity.
[0100] 3. It can be seen from Example 1 and Comparative Example 1 that after increasing the temperature of the hot pressing sintering, the bending strength and electrical conductivity of the target material decreased to varying degrees compared with Example 1, and the electrical conductivity decreased particularly seriously. The reason is that the amount of zinc aluminate generated under high temperature increases, which leads to a decrease in the electrical conductivity of the target material;
[0101] Further observation of Comparative Example 2 shows that when the temperature remains unchanged but sintering is not performed under pressure, the bending strength and electrical conductivity of the target material of Comparative Example 2 both show a significant downward trend. The reason is that at the same temperature, when the pressure is removed, the reaction is difficult to proceed completely, which leads to uneven components inside the target material, thereby reducing the density and electrical conductivity of the target material.
[0102] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a zinc oxide target, characterized in that: The following steps are involved: Step 1: Mix zinc oxide powder, aluminum oxide powder and gallium oxide powder, and spray granulate to obtain powder; Step 2: hot pressing and sintering the powder obtained in step 1 once, hot pressing and sintering twice, and then cooling and reducing pressure to obtain a zinc oxide target; During the primary hot pressing sintering process, the temperature is 400-600°C and the pressure is 2-4MPa; During the secondary hot pressing sintering process, the temperature is 1200-1300° C. and the pressure is 20-30 MPa.
2. The method for preparing a zinc oxide target according to claim 1, characterized in that: The mass ratio of the zinc oxide powder, the aluminum oxide powder and the gallium oxide powder is 96-98.5:1-3:0.5-1.
3. The method for preparing a zinc oxide target according to claim 1, characterized in that: In the step 1, the powder obtained by spray granulation includes powder 1 and powder 2, the average particle size of powder 1 is 25 to 60 μm, and the average particle size of powder 2 is 60 to 90 μm and does not include 60 μm.
4. The method for preparing a zinc oxide target according to claim 3, characterized in that: The step 1 is specifically as follows: Firstly, zinc oxide powder and aluminum oxide powder are mixed and spray granulated to obtain powder 1; Then, zinc oxide powder and gallium oxide powder are mixed and spray granulated to obtain powder 2; In the powder 1 and the powder 2, the mass ratio of zinc oxide is 1:4-5.
5. The method for preparing a zinc oxide target according to claim 1, characterized in that: The step 2 is performed in a vacuum environment, and the vacuum degree of the vacuum environment is not higher than 10Pa.
6. The method for preparing a zinc oxide target according to claim 1, characterized in that: The primary hot pressing sintering is specifically as follows: placing the powder obtained in step 1 in a vacuum environment, first heating the temperature to 400-600° C. at a heating rate of 0.5-1° C. / min, while increasing the pressure to 2-4 MPa, and maintaining the temperature and pressure for 1.5-3 hours; The secondary hot pressing sintering is specifically as follows: the material that has completed the primary sintering is heated to 1200-1300° C. at a heating rate of 1-2° C. / min, and the pressure is increased to 20-30 MPa, and the temperature and pressure are maintained for 4-6 hours.
7. A zinc oxide target, characterized in that: The target is prepared by the method for preparing the zinc oxide target described in any one of claims 1 to 5.
8. The zinc oxide target according to claim 7, characterized in that The flexural strength of the zinc oxide target material is not less than 140 MPa, and the electrical conductivity is not less than 500 s / cm.
Citation Information
Patent Citations
Aluminum-gallium co-doping zinc oxide nano-powder and preparation method for high intensity high conductivity sputtering coating target material thereof
CN103408062A
Gallium-aluminum-doped zinc oxide target material as well as preparation method and application thereof
CN116751048A
Zinc-gallium-aluminum ternary oxide rotary ceramic target and preparation method thereof
CN103695849A
Preparation method of high-purity oxide for manufacturing target material
CN114853465A
High-density high-uniformity zinc aluminum oxide target material and preparation method thereof
CN117209267A