Preparation of cellulose carboxylic acid monoester lithium and application of cellulose carboxylic acid monoester lithium as lithium battery electrode binder

As the electrode adhesive of lithium cellulose carboxylic acid prepared by solvent-free ball milling, it solves the problems of insufficient adhesion and preparation complexity of existing electrode adhesives, and achieves efficient and environmentally friendly electrochemical performance and cycle stability reduces irreversible lithium ion losses and meets the requirements of lithium battery electrode materials.

CN118930665APending Publication Date: 2024-11-12GUIZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411239054.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the use of existing lithium-ion battery electrode adhesives, there are problems such as insufficient adhesion, complex preparation process, high cost and potential environmental hazards, and irreversible lithium ion loss during recycling, resulting in a decrease in capacity.

Method used

The solvent-free ball milling method is used to prepare lithium cellulose carboxylic acid monoester as electrode binder, and lithium salt is used as catalyst and lithium source to improve the modifiability of cellulose through ball milling method, and combine it with water to form high efficiency. , environmentally friendly electrode adhesive.

Benefits of technology

The electrode is highly adhesion, good electrochemical performance and cycle stability, significantly reduces irreversible capacity loss, improves the lithium ion diffusion rate and battery cycle life, and has a simple process, low cost and no solvent participation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930665A_ABST
    Figure CN118930665A_ABST
Patent Text Reader

Abstract

The invention discloses a water-soluble cellulose carboxylic acid monoester lithium prepared by taking cellulose and cyclic carboxylic acid anhydride as raw materials and a lithium salt as a catalyst through a ball milling mode under a solvent-free condition, an application of the water-soluble cellulose carboxylic acid monoester lithium as a lithium battery electrode adhesive and the lithium battery electrode adhesive. The cellulose carboxylic acid monoester lithium adhesive disclosed by the invention is beneficial to the cycling stability of a lithium battery and can be used for different lithium battery electrode materials, and meanwhile, the whole preparation process of the aqueous cellulose-based adhesive disclosed by the invention is efficient, green and good in atom economy. The obtained product has the advantages of favorable water solubility, no toxicity, environment friendliness, high safety, low cost and simple preparation method, can be used as a lithium battery electrode material, can reduce the loss of irreversible capacity, can guide the formation of a uniform and stable interface solid electrolyte layer, and greatly enhances the lithium ion diffusion rate and cycle life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium battery electrode binder and an electrode material, in particular to the preparation of cellulose carboxylic acid monoester lithium and its application as a lithium battery electrode binder. Background Art

[0002] Due to the growing demand for energy in the past few decades, the vigorous development and utilization of renewable energy has aroused extensive research on energy storage devices. Among them, lithium-ion batteries have become one of the most important energy storage devices due to their light weight and high energy density. Since their first commercialization in 1991, lithium-ion batteries have been widely used in various mobile devices, electric vehicles and smart grid systems.

[0003] Polymers are commonly used ingredients in lithium-ion batteries and are widely used in the fields of electrolytes, separators, and electrode binders. In particular, although the proportion of electrode binders in batteries is low, they play a key role at the electrode interface and have a key role in the cycle life and irreversible capacity loss of batteries. Therefore, the development of functional binders for cathodes and anodes has attracted widespread attention.

[0004] The main function of the polymer binder is to maintain the integrity of the electrode and to bond the active material with the conductive component to the current collector. The basic requirements of the polymer binder include high adhesion and chemical stability, good mechanical strength and good electrochemical stability. Polyvinylidene fluoride (PVDF) is the most common commercial electrode binder for lithium-ion batteries due to its good electrochemical and mechanical stability, but its adhesion is mainly provided by van der Waals forces, so its adhesion is weak. At the same time, it is inert to the conduction of lithium ions and has high polarization resistance under high charge and discharge. Based on this, researchers have improved the performance by grafting and modifying PVDF. For example, in patent CN144566648B, PVDF is grafted with alkenyl ionic liquid, vinyl trisbutyl oxime silane, and lithium acrylate to obtain a modified PVDF-based binder, which improves the bonding strength. At the same time, due to the introduction of different hydrophilic and hydrophobic monomers, the high swelling rate of PVDF in the electrolyte is reduced, making it difficult to lose active substances. However, the preparation of PVDF slurry requires the use of N-methyl-pyrrolidone (NMP) solvent, which leads to high manufacturing costs and inherent environmental, safety and health (ESH) issues. Therefore, various studies have focused on developing cheaper, water-soluble, more environmentally friendly and easy-to-process polymer binders, such as patent CN116053480A, which uses a water slurry of sodium polyacrylate and polytetrafluoroethylene as a binder to improve the dispersion effect of the conductive agent, thereby reducing the content of the conductive agent and increasing the content of the active substance, while significantly improving the liquid absorption capacity of the electrode sheet.

[0005] Cellulose will play a key role in the development of sustainable electrochemical energy storage systems due to its wide sources, high abundance, low cost, easy recovery and environmentally acceptable properties. It is also widely used in adhesives. For example, carboxymethyl cellulose (CMC) has been widely studied. For example, in patent CN108473594B, cellulose is alkalized, etherified, refined, crushed, etc. through multiple processes to obtain an electrode adhesive, which suppresses defects on the electrode surface such as pinholes, and the battery using the modified adhesive has excellent capacity retention. Since lithium-ion batteries will inevitably generate "dead lithium" during the recycling process, causing irreversible lithium loss, researchers have proposed a lithium-supplementing adhesive mechanism. Lithium ions are introduced into many adhesives to improve the reversible capacity. Adding lithium-containing compounds to electrodes is a more appropriate strategy, and the introduction of lithium ions into electrode adhesives has attracted people's attention. For example, patents CN110767880A and CN104409737B both introduce lithium-containing compounds into the adhesive, which significantly improves the performance of the electrode. However, most of these water-based adhesives are not ideal when used as lithium battery electrode adhesives. They require multi-component mixing to improve various performances such as dispersion, slurry stability, coating stability, and electrode adhesion. The preparation process is complicated, and the process of introducing lithium ions requires the use of solvents. The components are numerous and the cost is high.

[0006] Based on this, in order to develop a water-based adhesive for lithium battery electrodes with a simple preparation process and low cost, the technicians of the present invention prepared a cellulose carboxylic acid monoester lithium adhesive by a solvent-free ball milling method, in which the lithium salt not only serves as a catalyst to make the cellulose have good modifiability, but also serves as a lithium source for the lithium-supplementing adhesive. Compared with the traditional solvent-based grafting modification of cellulose, the entire preparation process of the present invention is green, efficient and solvent-free, and the ball-milled product can be dispersed in water and used directly as an adhesive, and further purified to obtain an adhesive with better performance and high atomic economy. In addition, the cellulose carboxylic acid monoester lithium adhesive prepared by ball milling can not only improve its dispersibility for active materials, but also improve the apparent diffusion coefficient of lithium ions in the electrode. By introducing lithium ions into the adhesive, the lithium loss in the cyclic charge and discharge process is supplemented, the irreversible capacity is reduced, the electrochemical performance of the electrode is improved, and the battery cycle stability is significantly improved. The capacity loss of each cycle is less than 0.01%, which meets the requirements of the preparation process of lithium battery electrode materials. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a preparation of cellulose carboxylic acid monoester lithium and its application as a lithium battery electrode binder. The cellulose carboxylic acid monoester lithium of the present invention is prepared by ball milling under solvent-free conditions, and the process is simple; when used as a binder, water is used as a solvent, and it has the advantages of being non-toxic and environmentally friendly, highly safe, low-cost, and simple in preparation method. When used in lithium batteries, it can guide the formation of a uniform interfacial solid electrolyte layer, supplement the irreversible capacity loss in the first lithium insertion process, and greatly improve the battery lithium ion diffusion rate and cycle life.

[0008] One of the technical solutions of the present invention:

[0009] Provided is a cellulose carboxylic acid monoester lithium, which is obtained by taking cellulose as a raw material, adding a cyclic acid anhydride and a lithium-containing compound, ball milling for 2-24 hours, and dialysis purification.

[0010] Preferably, in the aforementioned cellulose carboxylic acid monoester lithium, the molar ratio of the hydroxyl group in the cellulose, the anhydride in the cyclic carboxylic acid anhydride and the lithium in the lithium-containing compound is 1:1:1; and the degree of substitution of the cellulose carboxylic acid monoester lithium is 0.5-1.5.

[0011] Preferably, in the aforementioned cellulose carboxylic acid monoester lithium, the cellulose is one or any combination of microcrystalline cellulose, cotton, wood pulp, bamboo pulp or plant cellulose separated from agricultural and forestry lignocellulose waste.

[0012] Preferably, in the aforementioned cellulose carboxylic acid monoester lithium, the cyclic carboxylic anhydride is one or any combination of maleic anhydride, itaconic anhydride, tetrafluorosuccinic anhydride, diglycolic anhydride, glutaric anhydride, butylsuccinic anhydride, succinic anhydride, adipic anhydride, 2-methylsuccinic anhydride, n-octylsuccinic anhydride or allylsuccinic anhydride.

[0013] The second technical solution of the present invention:

[0014] Provided is an application of cellulose carboxylic acid monoester lithium as a lithium battery electrode binder.

[0015] The third technical solution of the present invention:

[0016] Provided is a lithium battery electrode binder, comprising the above-mentioned cellulose carboxylic acid monoester lithium.

[0017] Preferably, the preparation method of the aforementioned lithium battery electrode adhesive is to directly dissolve the cellulose carboxylic acid monoester lithium in water to obtain the lithium battery electrode adhesive; wherein the mass ratio of the cellulose carboxylic acid monoester lithium to water is 5:80-100.

[0018] The fourth technical solution of the present invention:

[0019] Provided is a lithium battery electrode, which contains the lithium battery electrode binder mentioned above.

[0020] Preferably, the aforementioned lithium battery electrode is prepared by uniformly mixing the lithium battery electrode material, the conductive agent and the lithium battery electrode binder to obtain an electrode slurry, and then drying the electrode slurry to obtain the lithium battery electrode.

[0021] Preferably, in the aforementioned lithium battery electrode, the electrode material is any one of lithium iron phosphate, lithium manganese oxide, a ternary electrode material or lithium cobalt oxide.

[0022] Preferably, for the aforementioned lithium battery electrode, the drying is to coat the electrode slurry on a carbon-coated aluminum foil and dry it in vacuum at 80-120° C. for 8-24 hours.

[0023] Beneficial effects of the present invention:

[0024] 1. The cellulose carboxylic acid monoester lithium of the present invention is prepared by ball milling under solvent-free conditions, which has a simple process and is easy to implement industrially.

[0025] 2. When the cellulose carboxylic acid monoester lithium of the present invention is used as a binder, water is used as the binder, it is directly dissolved in deionized water and directly used as a lithium battery electrode binder, which has the advantages of being non-toxic and environmentally friendly, highly safe, low-cost and having a simple preparation method.

[0026] 3. When the cellulose carboxylic acid monoester lithium of the present invention is used as an adhesive, the strong hydrogen bond network structure in cellulose gives the adhesive higher adhesion; at the same time, due to the special structure of the cellulose carboxylic acid monoester lithium, lithium ions are introduced to reduce the irreversible capacity of the lithium battery.

[0027] 4. When the cellulose carboxylic acid monoester lithium of the present invention is used as a binder, it can effectively reduce the interface impedance of the electrode, greatly improve the diffusion rate of lithium ions in the battery, and further affect the entire lithium ion extraction / insertion process in the electrode, so that it has good rate performance.

[0028] 5. When the cellulose carboxylic acid monoester lithium of the present invention is used as a binder, it can guide the formation of a uniform interfacial solid electrolyte layer, while keeping most of the active materials always adhered to the electrode current collector, greatly improving its cycle stability.

[0029] In summary, the lithium salt in the preparation method of cellulose carboxylic acid monoester lithium of the present invention not only acts as a catalyst to make cellulose have good modifiability, but also serves as a lithium source for lithium-supplementing adhesives. Moreover, the entire preparation process of the present invention is green, efficient, and solvent-free. The product after ball milling can be dispersed in water and used directly as an adhesive, and further purified to obtain an adhesive with better performance and high atom economy. At the same time, the method of the present invention prepares cellulose carboxylic acid monoester lithium by ball milling, which can not only improve its dispersibility to active materials, but also improve the apparent diffusion coefficient of lithium ions in the electrode. By introducing lithium ions into the adhesive, the lithium loss in the cyclic charge and discharge process is supplemented, the irreversible capacity is reduced, the electrochemical performance of the electrode is improved, and the battery cycle stability is significantly improved. The capacity loss of each cycle is less than 0.01%, which meets the requirements of the preparation process of lithium battery electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The positive lithium iron phosphate materials obtained in Example 1, Example 2 and Comparative Example 1 and Comparative Example 2 of the present invention are assembled into a long cycle diagram of a lithium battery. Example 1 shows a high capacity retention rate of 98% after 300 cycles at 0.5C, Example 2 shows a high capacity retention rate of 85%, and the capacity retention rates of Comparative Example 1 and Comparative Example 2 are 74% and 82% respectively after 300 cycles at 0.5C.

[0031] Figure 2 The positive lithium iron phosphate materials obtained in Example 1 and Example 2 of the present invention and Comparative Examples 1 and 2 are used to assemble the rate cycle diagram of the lithium battery. Example 1 shows high rate performance of 160.7 mAh / g, 159.6 mAh / g, 153.1 mAh / g, 144.2 mAh / g, 129.4 mAh / g, 118.5 mAh / g, and 99.5 mAh / g at 0.1C, 0.2C, 0.5C, 1C, 2C, 3C, and 6C, respectively; Example 2 shows high rate performance of 160.9 mAh / g, 159.0 mAh / g, 150.1 mAh / g, 140.6 mAh / g, 126.8 mAh / g, 112.9 mAh / g, and 90.4 mAh / g at 0.1C, 0.2C, 0.5C, 1C, 2C, 3C, and 6C, respectively, while Comparative Examples 1 and 2 have poor rate performance.

[0032] Figure 3 In Example 3 of the present invention, the present invention is used as a binder for the ternary positive electrode material NMC811, and the long cycle diagram of the assembled lithium battery also has high cycle stability.

[0033] Figure 4In Example 4 of the present invention, the present invention is used as a binder for lithium manganese oxide (LMO), and a long cycle diagram of the assembled lithium battery is obtained, which also has high cycle stability.

[0034] Figure 5 The positive electrode lithium iron phosphate materials obtained in Example 1 of the present invention and Comparative Examples 1 and 2 are used to assemble lithium batteries for 100 cycles. From the scanning electron microscope images of the interfacial solid electrolyte layer formed on the surface of the materials, it can be clearly found that after the cycle, the morphology of the electrode of Example 1 is more complete, while a large number of cracks appear in Comparative Examples 1 and 2, and the loss of active materials is more serious.

[0035] Figure 6 The positive electrode lithium iron phosphate material obtained in Example 1 of the present invention and Comparative Examples 1 and 2 is a transmission electron microscope image of the interface solid electrolyte layer formed on the surface of the material after 100 cycles of the assembled lithium metal battery. It can be clearly found that the solid electrolyte layer of Example 1 after the cycle is thinner and more uniform than that of the comparative example, and the component distribution is uniform and stable. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0037] Embodiments of the present invention

[0038] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0039] Unless otherwise specified, the reagents and materials used in the following examples can be obtained from commercial sources.

[0040] The battery performance tests in the following embodiments are all conducted using the Chenhua battery testing system. In the following embodiments, the lithium sheet is used as the negative electrode, the electrode material made of the prepared adhesive is used as the positive electrode, polyethylene (PE) is used as the separator, and the electrolyte is 1MLiFP6 dissolved in EC:EMC:DMC=1:1:1wt%. CR2032 button batteries are assembled in an argon atmosphere, and the electrochemical capacity, rate performance and stability are tested at constant current density and different current density.

[0041] The cellulose lithium succinate in the following examples was prepared by the following method:

[0042] 1) Mix microcrystalline cellulose and lithium hydroxide in a molar ratio of hydroxyl group to lithium of 1:1, add into a ball mill, add 400 g of agate balls, and perform ball milling activation for 2 h at room temperature and 500 r / min to obtain lithium-containing activated cellulose powder;

[0043] 2) adding succinic anhydride to the cellulose powder so that the molar ratio of anhydride to hydroxyl groups in microcrystalline cellulose is 1:1, and subjecting the mixture to ball milling reaction at room temperature for 12 hours to obtain a powder mixture of cellulose lithium succinate, succinate and lithium-containing compound;

[0044] 3) The cellulose lithium succinate powder mixture is directly dialyzed and freeze-dried to obtain cellulose lithium succinate.

[0045] Comparative Example 1

[0046] Put 0.3g of polyvinylidene fluoride (PVDF) powder into a glass bottle, add 10ml of NMP solvent, stir magnetically at room temperature, 500r / min, for 8h until completely dissolved, add 2.4g of lithium iron phosphate powder and 0.3g of acetylene black and the above PVDF solution for ball milling, coat on carbon-coated aluminum foil, and vacuum dry at 100℃ for 12h to obtain the positive electrode material.

[0047] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte and assembled into CR2032 button cells in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0048] Comparative Example 2

[0049] Put 0.1g carboxymethyl cellulose (CMC) powder into a glass bottle, add 10ml pure water, and stir magnetically at room temperature at 500r / min for 12h until it is completely dissolved. Add 0.8g lithium iron phosphate powder and 0.3g acetylene black and mix with the above CMC solution by ball milling, then coat on carbon-coated aluminum foil and dry in vacuum at 100℃ for 12h to obtain the electrode material.

[0050] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte and assembled into CR2032 button cells in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0051] Example 1

[0052] Put 0.5g of cellulose lithium succinate (CSAL, degree of substitution 0.8) powder into a glass bottle, add 10ml of pure water, stir magnetically at 50℃, 500r / min, and stir for 0.5h until completely dissolved, add 4g of lithium iron phosphate powder and 0.5g of acetylene black and the above-mentioned CSAL solution for ball milling, coat it on carbon-coated aluminum foil, and vacuum dry it at 100℃ for 12h to obtain the positive electrode material.

[0053] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte and assembled into CR2032 button cells in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0054] Example 2

[0055] Put 0.5g of cellulose lithium succinate (CSAL, degree of substitution 1.1) powder into a glass bottle, add 10ml of pure water, stir magnetically at 50℃, 500r / min, and stir for 0.5h until completely dissolved, add 4g of lithium iron phosphate powder and 0.5g of acetylene black and the above-mentioned CSAL solution for ball milling, coat it on carbon-coated aluminum foil, and vacuum dry it at 100℃ for 12h to obtain the positive electrode material.

[0056] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte and assembled into CR2032 button cells in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0057] Example 3

[0058] Put 0.125g of cellulose lithium succinate (CSAL, degree of substitution 0.8) powder into a glass bottle, add 2.5ml of pure water, stir magnetically at 50℃, 500r / min, and stir for 0.5h until completely dissolved, add 1g of NCM811 powder and 0.125g of acetylene black and the above-mentioned CSAL solution for ball milling, coat it on carbon-coated aluminum foil, and vacuum dry it at 100℃ for 12h to obtain the positive electrode material.

[0059] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte, and CR2032 button cells were assembled in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0060] Example 4

[0061] 0.125 g of cellulose lithium succinate (CSAL, degree of substitution 0.8) powder was put into a glass bottle, 2.5 ml of pure water was added, and magnetic stirring was performed at 50°C, 500 r / min, and the mixture was completely dissolved for 0.5 h. 1 g of LMO powder and 0.125 g of acetylene black were added to the above CSAL solution and ball-milled and mixed, and then coated on a carbon-coated aluminum foil and vacuum dried at 100°C for 12 h to obtain the positive electrode material.

[0062] 1MLiFP6 was dissolved in EC:EMC:DMC=1:1:1wt.% as the electrolyte and assembled into CR2032 button cells in an argon atmosphere. The electrochemical capacity, rate performance and long cycle stability were tested at constant current density and different current densities.

[0063] Example 5

[0064] Put cellulose lithium succinate powder into a glass bottle, add pure water at a mass ratio of cellulose lithium succinate: water = 5:95, stir with a magnetic stirrer at 50°C and 500r / min until it is completely dissolved to obtain an adhesive;

[0065] Lithium iron phosphate powder, a binder and acetylene black were mixed in a mass ratio of 8:1:1 and ball-milled, then coated on a carbon-coated aluminum foil and vacuum-dried at 100° C. for 10 h to obtain a positive electrode material.

[0066] Example 6

[0067] Put cellulose lithium succinate powder into a glass bottle, add pure water at a mass ratio of cellulose lithium succinate: water = 5:90, stir with a magnetic stirrer at 50°C and 500r / min until it is completely dissolved to obtain an adhesive;

[0068] Lithium iron phosphate powder, binder and conductive carbon black were mixed in a mass ratio of 8:1.5:0.5 and ball-milled, then coated on a carbon-coated aluminum foil and vacuum-dried at 100° C. for 12 h to obtain a positive electrode material.

[0069] Example 7

[0070] Put cellulose lithium succinate powder into a glass bottle, add pure water at a mass ratio of cellulose lithium succinate: water = 5:85, stir magnetically at 50°C, 500r / min, until completely dissolved, to obtain an adhesive;

[0071] The binder, lithium iron phosphate powder and acetylene black were mixed in a mass ratio of 8:0.5:1.5 and ball-milled, and then coated on a carbon-coated aluminum foil and vacuum-dried at 100° C. for 12 h to obtain a positive electrode material.

[0072] Example 8

[0073] Put cellulose lithium succinate powder into a glass bottle, add pure water at a mass ratio of cellulose lithium succinate: water = 5:80, stir magnetically at 50°C, 500r / min, until completely dissolved, to obtain an adhesive;

[0074] The binder, lithium iron phosphate powder and acetylene black were mixed in a mass ratio of 8:1:1 and ball-milled, and then coated on a carbon-coated aluminum foil and vacuum-dried at 80° C. for 24 hours to obtain a positive electrode material.

[0075] Example 9

[0076] Put cellulose lithium succinate powder into a glass bottle, add pure water at a mass ratio of cellulose lithium succinate: water = 5:80, stir magnetically at 50°C, 500r / min, until completely dissolved, to obtain an adhesive;

[0077] The binder, lithium iron phosphate powder and acetylene black were mixed in a mass ratio of 8:1.5:0.5 and ball-milled, and then coated on a carbon-coated aluminum foil and vacuum-dried at 120° C. for 8 h to obtain a positive electrode material.

[0078] Example 10

[0079] 1) Cotton and lithium hydroxide were mixed in a molar ratio of hydroxyl to lithium of 1:1, added into a ball mill, 400 g of agate balls were added, the temperature was room temperature, ball milling reaction was activated for 12 h, the reaction condition was 500 r / min, and lithium-containing activated cellulose powder was obtained;

[0080] 2) adding maleic anhydride to the cellulose powder so that the molar ratio of the anhydride to the hydroxyl group in the microcrystalline cellulose is 1:1, and subjecting the mixture to ball milling reaction at room temperature for 12 hours to obtain a mixture of cellulose maleate lithium, maleate and lithium-containing compound powders;

[0081] 3) The cellulose maleate lithium powder mixture is directly dialyzed and freeze-dried to obtain cellulose maleate lithium.

[0082] Embodiment 11

[0083] 1) Mix wood pulp and lithium hydroxide in a molar ratio of hydroxyl to lithium of 1:1, add into a ball mill, add 400 g of agate balls, and perform ball milling activation for 2 h at room temperature and 500 r / min to obtain lithium-containing activated cellulose powder;

[0084] 2) adding diglycolic anhydride to the cellulose powder so that the molar ratio of the anhydride to the hydroxyl group in the microcrystalline cellulose is 1:1, and subjecting the mixture to ball milling reaction at room temperature for 12 hours to obtain a mixture of cellulose diglycolic acid lithium, diglycolic acid ester and lithium-containing compound powder;

[0085] 3) The cellulose diglycolate lithium powder mixture is directly dialyzed and freeze-dried to obtain cellulose diglycolate lithium.

[0086] Example 12

[0087] 1) bamboo pulp and lithium hydroxide were mixed in a molar ratio of hydroxyl group to lithium of 1:1, added into a ball mill, 400 g of agate balls were added, the temperature was room temperature, ball milling reaction was activated for 24 h, the reaction condition was 500 r / min, and lithium-containing activated cellulose powder was obtained;

[0088] 2) adding allyl succinic anhydride to the cellulose powder so that the molar ratio of the anhydride to the hydroxyl group in the microcrystalline cellulose is 1:1, and subjecting the mixture to ball milling reaction at room temperature for 12 hours to obtain a mixture of cellulose allyl succinate lithium, allyl succinate and lithium-containing compound powders;

[0089] 3) The cellulose allyl succinate lithium powder mixture is directly dialyzed and freeze-dried to obtain cellulose allyl succinate lithium.

[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A cellulose carboxylic acid monoester lithium, characterized in that: The cellulose is used as a raw material, and cyclic carboxylic acid anhydride and a lithium-containing compound are added, ball milled for 2-24 hours, and then purified by dialysis.

2. The cellulose carboxylic acid monoester lithium according to claim 1, characterized in that: The molar ratio of the hydroxyl group in the cellulose, the anhydride in the cyclic carboxylic anhydride and the lithium in the lithium-containing compound is 1:1:1; and the degree of substitution of the lithium monoester of cellulose carboxylic acid is 0.5-1.

5.

3. The cellulose carboxylic acid monoester lithium according to claim 1, characterized in that: The cellulose is one or any combination of microcrystalline cellulose, cotton, wood pulp, bamboo pulp or plant cellulose separated from agricultural and forestry lignocellulose waste.

4. The cellulose carboxylic acid monoester lithium according to claim 1, characterized in that: The cyclic carboxylic anhydride is one or any combination of maleic anhydride, itaconic anhydride, tetrafluorosuccinic anhydride, diglycolic anhydride, glutaric anhydride, butylsuccinic anhydride, succinic anhydride, adipic anhydride, 2-methylsuccinic anhydride, n-octylsuccinic anhydride or allylsuccinic anhydride.

5. Use of the cellulose carboxylic acid monoester lithium according to any one of claims 1 to 4 as a lithium battery electrode binder.

6. A lithium battery electrode adhesive, characterized in that: The cellulose carboxylic acid monoester lithium is contained in any one of claims 1 to 4.

7. The lithium battery electrode binder according to claim 6, characterized in that: The preparation method is to directly dissolve the cellulose carboxylic acid monoester lithium in water, and then obtain a lithium battery electrode adhesive; wherein the mass ratio of the cellulose carboxylic acid monoester lithium to water is 5:80-100.

8. A lithium battery electrode, characterized in that: It contains the lithium battery electrode binder according to claim 6 or 7.

9. The lithium battery electrode according to claim 8, characterized in that: The preparation method comprises the following steps: uniformly mixing the lithium battery electrode material, the conductive agent and the lithium battery electrode adhesive to obtain an electrode slurry, then coating the electrode slurry on a carbon-coated aluminum foil, and vacuum drying at 80-120° C. for 8-24 hours to obtain a lithium battery electrode.

10. The lithium battery electrode according to claim 9, characterized in that: The electrode material is any one of lithium iron phosphate, lithium manganese oxide, a ternary electrode material or lithium cobalt oxide.