Alkali-soluble UV (Ultraviolet) resin as well as preparation method and application thereof

By using alkali-soluble UV resin in low-temperature sintered silver paste, the problem of unstable performance of traditional silver paste is solved, high exposure depth and low-temperature sintering are achieved, and the conductivity and resolution of silver paste are improved.

CN118930725APending Publication Date: 2024-11-12QIANYU ELECTRONIC MATERIALS (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174410.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In low-temperature sintered silver paste, traditional silver powder has darker color and is extremely difficult to expose. The exposure and dispersion of resins lead to unstable performance of silver paste, affecting its performance in electronic materials and other fields.

Method used

Using an alkali-soluble UV resin preparation method, through copolymerization reaction, acrylic compound modification and acid anhydride compound modification, UV resin with excellent photosensitive activity and alkali-soluble is obtained, which is used to increase the exposure depth and sintering temperature of silver powder. Achieve low-temperature sintering.

Benefits of technology

It effectively improves the exposure depth and conductivity of silver paste, reduces the sintering temperature, improves the density and resolution of cross-linking network, and enhances the performance stability of silver paste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930725A_ABST
    Figure CN118930725A_ABST
Patent Text Reader

Abstract

The invention discloses alkali-soluble UV (ultraviolet) resin and a preparation method and application thereof, and belongs to the technical field of electronics. First, a first monomer, a second monomer and a third monomer are copolymerized, then modified with an olefine acid compound and finally modified with an anhydride compound, and the alkali-soluble UV resin is obtained. The alkali-soluble UV resin has excellent photosensitive activity and alkali solubility, the exposure depth of silver powder in the silver paste can be effectively improved, the sintering temperature can be effectively reduced, sintering can be completed at the low temperature (lower than 200 DEG C), the silver powder can be effectively wetted and dispersed, the cross-linked network density is improved, and the conductivity and the resolution ratio of the silver paste are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic materials, and in particular to an alkali-soluble UV resin and a preparation method and application thereof. Background Art

[0002] In the fields of electronic materials, solar panels, touch screens, etc., silver paste is an important conductive material and its performance directly affects the performance and quality of the products.

[0003] In low-temperature sintering silver paste, the silver powder commonly used has a low average particle size, and the color of nanosilver is darker and has strong light-shielding properties, which makes the exposure of the silver paste extremely difficult and the exposure depth is shallow. In the traditional silver paste preparation process, due to the exposure and solubility and dispersion problems of the resin, the performance of the silver paste is often unstable, affecting its performance in various applications.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an alkali-soluble UV resin and a preparation method and application thereof. The alkali-soluble UV resin has excellent photosensitivity and alkali solubility, can effectively increase the exposure depth of silver powder in silver paste, effectively reduce the sintering temperature, complete sintering at a low temperature (below 200°C), effectively wet and disperse the silver powder, increase the cross-linking network density, and effectively improve the conductivity and resolution of the silver paste.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0008] (1) mixing the first monomer, the second monomer, the third monomer, the initiator, and the molecular weight regulator uniformly, adding the mixture to a solvent, and reacting the mixture under a protective atmosphere at a first temperature for 1 to 4 hours, then at a second temperature for 0.5 to 2 hours, and finally at a third temperature for 0.5 to 2 hours to obtain a copolymer solution;

[0009] (2) mixing the olefinic acid compound, the polymerization inhibitor and the catalyst uniformly, adding the mixture to the copolymer solution, reacting the mixture at 80 to 110° C. in an oxygen atmosphere until the acid value drops below 5 mgKOH / g, thereby obtaining a modified copolymer solution;

[0010] (3) adding an acid anhydride compound to the modified copolymer solution and reacting at 80 to 120° C. to obtain an alkali-soluble UV resin;

[0011] The first monomer includes at least one of isobornyl methacrylate, isobornyl acrylate, acryloyl morpholine, and styrene;

[0012] The second monomer includes at least one of glycidyl methacrylate and glycidyl acrylate;

[0013] The structural formula of the third monomer is shown in Formula I:

[0014]

[0015] In formula I, R1 is hydrogen or methyl; R2 is (CH2) n CH3 or at least one of the following groups:

[0016]

[0017] n is an integer from 0 to 18.

[0018] The present invention first copolymerizes a first monomer, a second monomer and a third monomer, then modifies them with an olefinic acid compound, and finally modifies them with an acid anhydride compound to obtain an alkali-soluble UV resin. The alkali-soluble UV resin has excellent photosensitivity and alkali solubility, can effectively improve the exposure depth of silver powder in silver paste, effectively reduce the sintering temperature, can complete sintering at a low temperature (below 200° C.), effectively wets and disperses silver powder, improves the cross-linking network density, and effectively improves the conductivity and resolution of the silver paste.

[0019] As a preferred embodiment of the present invention, the mass ratio of the first monomer, the second monomer, the third monomer, the initiator, the molecular weight regulator and the solvent is (5-15): (15-40): (5-25): (0.5-2): (0.1-1.5): (30-65).

[0020] As a preferred embodiment of the present invention, the molecular weight regulator includes at least one of 3-mercaptopropionate, tert-dodecyl mercaptan, n-dodecyl mercaptan, secondary dodecyl mercaptan, and mercaptoethanol;

[0021] The initiator comprises at least one of diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide, di-tert-amyl peroxide, diisopropyl peroxide, and di-tert-butyl peroxide;

[0022] The solvent includes at least one of isophorone, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ester, propylene glycol methyl ether, trimethylbenzene, and tetramethylbenzene.

[0023] As a preferred embodiment of the present invention, the olefinic acid compound includes at least one of 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid, 1,6-heptadiene-4-carboxylic acid, acrylic acid, and methacrylic acid;

[0024] The polymerization inhibitor is at least one of p-methoxyphenol, 2,6-di-tert-butyl-4-methylphenol, hydroquinone, p-tert-butylcatechol or 2,6-dinitro-p-cresol;

[0025] The catalyst is at least one of benzyldimethylamine, triphenylphosphine, aluminum acetylacetonate, tetrabutylammonium bromide, tetraethylammonium bromide, benzyltriethylammonium chloride and triethylamine;

[0026] The acid anhydride compound includes at least one of phthalic anhydride, dodecyl succinic anhydride, methyl nadic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0027] As a preferred embodiment of the present invention, the mass ratio of the copolymer solution, the olefinic acid compound, the polymerization inhibitor, and the catalyst is 100: (8-25): (0.04-2): (0.3-3);

[0028] The mass ratio of the acid anhydride compound to the modified copolymer solution is (8-20):100.

[0029] As a preferred embodiment of the present invention, the acid anhydride compound includes at least one of phthalic anhydride, dodecylsuccinic anhydride, methylnadic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0030] As a preferred embodiment of the present invention, the first temperature is T1°C, satisfying: 75°C≤T1≤110°C;

[0031] The second temperature is T2°C, satisfying 5°C≤T2-T1≤15°C;

[0032] The third temperature is T3°C, satisfying 10°C≤T3-T2≤15°C.

[0033] The invention also provides an application of an alkali-soluble UV resin in preparing a low-temperature sintering silver paste.

[0034] The present invention also provides a low-temperature sintering silver paste, comprising an alkali-soluble UV resin; the mass percentage of the alkali-soluble UV resin in the low-temperature sintering silver paste is 5 to 20%;

[0035] The alkali-soluble UV resin is the alkali-soluble UV resin described above.

[0036] As a preferred embodiment of the present invention, the low-temperature sintering silver paste also includes silver powder, and the silver powder is a first spherical silver powder and a second spherical silver powder, the average particle size of the first spherical silver powder is 0.2-5 μm, the average particle size of the second spherical silver powder is 20-80 nm, the mass ratio of the first spherical silver powder to the second spherical silver powder is (20-80): (20-80), and the mass percentage of the silver powder in low-temperature sintering is 70-90%.

[0037] As a preferred embodiment of the present invention, the low temperature sintering further comprises an auxiliary agent, and the mass percentage of the auxiliary agent in the low temperature sintering is 0.1-1%.

[0038] As a preferred embodiment of the present invention, the low-temperature sintering further comprises a diluent, and the diluent is hydroxyethyl methacrylate, and the mass percentage of the diluent in the low-temperature sintering is 0.5-4%.

[0039] As a preferred embodiment of the present invention, the low-temperature sintering further comprises epoxy resin, the epoxy resin is KD-242C, and the mass percentage of the epoxy resin in the low-temperature sintering is 0.2-1%.

[0040] As a preferred embodiment of the present invention, the low-temperature sintering further comprises a photoinitiator, and the photoinitiator is photoinitiator 819. The mass percentage of the photoinitiator in the low-temperature sintering is 0.5-2%.

[0041] As a preferred embodiment of the present invention, the low temperature sintering further comprises aluminum acetylacetonate, and the mass percentage of the aluminum acetylacetonate in the low temperature sintering is 0.002 to 0.02%.

[0042] Specifically, the low-temperature sintering comprises the following components in percentage by mass: 5-20% alkali-soluble UV resin, 70-90% silver powder, 0.5-4% diluent, 0.2-1% epoxy resin, 0.5-2% photoinitiator, 0.1-1% auxiliary agent, and 0.002-0.02% aluminum acetylacetonate.

[0043] The beneficial effects of the present invention are as follows: the present invention first copolymerizes the first monomer, the second monomer and the third monomer, then modifies them with an olefinic acid compound, and finally modifies them with an acid anhydride compound to obtain an alkali-soluble UV resin. The alkali-soluble UV resin has excellent photosensitivity and alkali solubility, can effectively improve the exposure depth of silver powder in the silver paste, effectively reduce the sintering temperature, can complete sintering at a low temperature (below 200° C.), effectively wets and disperses the silver powder, improves the cross-linking network density, and effectively improves the conductivity and resolution of the silver paste. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1This is the infrared spectrum of the resin synthesized in Example 1. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0046] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0047] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0048] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0049] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.

[0050] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0051] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0052] Example 1

[0053] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0054] (1) 10 parts by weight of isobornyl methacrylate, 30 parts by weight of glycidyl methacrylate, 15 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 85° C. for 2 h, then at 95° C. for 1 h, and finally at 107° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0055] The structural formula of the third monomer is shown in Formula I:

[0056]

[0057] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0058] (2) 15 parts by mass of 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid, 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were uniformly mixed, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours (the acid value dropped to less than 5 mgKOH / g) under an oxygen atmosphere to obtain a modified copolymer solution;

[0059] (3) 15 parts by mass of phthalic anhydride were added to 100 parts by mass of the modified copolymer solution, and the mixture was reacted at 100° C. for 4 hours (without any change in the acid value) to obtain an alkali-soluble UV resin.

[0060] The infrared spectrum of the alkali-soluble UV resin synthesized in this embodiment is as follows: Figure 1 As shown in the figure, it can be seen that 913cm -1 The characteristic peak of epoxy disappears, while the peak at 1632 cm -1 It is the characteristic peak of double bond at 1850cm -1 and 1750cm -1 There are no two coupling characteristic peaks of anhydride on the left and right, indicating that the synthesis reaction proceeds smoothly.

[0061] Example 2

[0062] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0063] (1) 15 parts by weight of isobornyl methacrylate, 15 parts by weight of glycidyl methacrylate, 5 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 75° C. for 2 h, then at 90° C. for 1 h, and finally at 105° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0064] The structural formula of the third monomer is shown in Formula I:

[0065]

[0066] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0067] (2) 20 parts by mass of 1,6-heptadiene-4-carboxylic acid (2-methylpent-4-enoic acid), 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were mixed uniformly, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours (the acid value dropped to less than 5 mgKOH / g) under an oxygen atmosphere to obtain a modified copolymer solution;

[0068] (3) 15 parts by mass of dodecyl succinic anhydride was added to 100 parts by mass of the modified copolymer solution, and the mixture was reacted at 100° C. for 4 h (without any change in the acid value) to obtain an alkali-soluble UV resin.

[0069] Example 3

[0070] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0071] (1) 5 parts by weight of isobornyl methacrylate, 40 parts by weight of glycidyl methacrylate, 25 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 100° C. for 2 h, then at 105° C. for 1 h, and finally at 115° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0072] The structural formula of the third monomer is shown in Formula I:

[0073]

[0074] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0075] (2) 25 parts by mass of 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid, 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were uniformly mixed, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours under an oxygen atmosphere (the acid value dropped to less than 5 mgKOH / g) to obtain a modified copolymer solution;

[0076] (3) 8 parts by mass of phthalic anhydride were added to 100 parts by mass of the modified copolymer solution, and the mixture was reacted at 100° C. for 4 hours (the acid value did not change), to obtain an alkali-soluble UV resin.

[0077] Example 4

[0078] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0079] (1) 10 parts by weight of isobornyl acrylate, 30 parts by weight of glycidyl acrylate, 15 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 85° C. for 2 h, then at 95° C. for 1 h, and finally at 107° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0080] The structural formula of the third monomer is shown in Formula I:

[0081]

[0082] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0083] (2) 15 parts by mass of 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid, 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were uniformly mixed, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours (the acid value dropped to less than 5 mgKOH / g) under an oxygen atmosphere to obtain a modified copolymer solution;

[0084] (3) 15 parts by weight of methyl nadic anhydride was added to 100 parts by weight of the modified copolymer solution, and the mixture was reacted at 100° C. for 4 h (without any change in the acid value) to obtain an alkali-soluble UV resin.

[0085] Comparative Example 1

[0086] The difference between Comparative Example 1 and Example 1 is that acrylic acid is used to replace 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid in Comparative Example 1, and the other contents are the same.

[0087] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0088] (1) 10 parts by weight of isobornyl methacrylate, 30 parts by weight of glycidyl methacrylate, 15 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 85° C. for 2 h, then at 95° C. for 1 h, and finally at 107° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0089] The structural formula of the third monomer is shown in Formula I:

[0090]

[0091] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0092] (2) 15 parts by mass of acrylic acid, 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were uniformly mixed, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours (the acid value dropped to less than 5 mgKOH / g) under an oxygen atmosphere to obtain a modified copolymer solution;

[0093] (3) 15 parts by mass of phthalic anhydride were added to 100 parts by mass of the modified copolymer solution, and the mixture was reacted at 100° C. for 4 hours (without any change in the acid value) to obtain an alkali-soluble UV resin.

[0094] Comparative Example 2

[0095] The difference between Comparative Example 2 and Example 1 is that the acid anhydride treatment is not used in Comparative Example 2, and the other aspects are the same.

[0096] A method for preparing a UV resin comprises the following steps:

[0097] (1) 10 parts by weight of isobornyl methacrylate, 30 parts by weight of glycidyl methacrylate, 15 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 85° C. for 2 h, then at 95° C. for 1 h, and finally at 107° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0098] The structural formula of the third monomer is shown in Formula I:

[0099]

[0100] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0101] (2) 15 parts by mass of acrylic acid, 0.5 parts by mass of p-methoxyphenol, and 1 part by mass of 2,6-di-tert-butyl-4-methylphenol were mixed uniformly, added to 100 parts by mass of the copolymer solution, and reacted at 90° C. for 5 hours (the acid value dropped to less than 5 mgKOH / g) under an oxygen atmosphere to obtain a UV resin.

[0102] Comparative Example 3

[0103] A method for preparing an alkali-soluble UV resin comprises the following steps:

[0104] (1) 10 parts by weight of isobornyl methacrylate, 30 parts by weight of glycidyl methacrylate, 15 parts by weight of a third monomer, 2 parts by weight of diisopropyl peroxydicarbonate, and 0.5 parts by weight of tert-dodecyl mercaptan were uniformly mixed, added to 50 parts by weight of ethylene glycol ethyl ether acetate, and reacted at 85° C. for 2 h, then at 95° C. for 1 h, and finally at 107° C. for 1 h under a nitrogen atmosphere to obtain a copolymer solution;

[0105] The structural formula of the third monomer is shown in Formula I:

[0106]

[0107] In formula I, R1 is hydrogen; R2 is C(CH3)3;

[0108] (2) 15 parts by mass of phthalic anhydride were added to 100 parts by mass of the copolymer solution, and the mixture was reacted at 100° C. for 4 hours (without any change in the acid value) to obtain an alkali-soluble UV resin.

[0109] Test Case

[0110] 1. Preparation of low temperature sintering:

[0111] (1) Weigh the following proportions: 10% alkali-soluble UV resin, 2% hydroxyethyl methacrylate, 0.6% epoxy resin KD-242C, 1% photoinitiator 819, 0.3% auxiliary agent, 0.01% aluminum acetylacetonate, and the remainder spherical silver powder; the spherical silver powder comprises a first spherical silver powder and a second spherical silver powder, the particle size of the first spherical silver powder is 1 μm, the average particle size of the second spherical silver powder is 50 nm, and the mass ratio of the first spherical silver powder to the second spherical silver powder is 50:50.

[0112] The auxiliary agent is composed of acrylated polysiloxane and trimethylsiloxane in a ratio of 1:1, and the acrylated polysiloxane is TEGO2100.

[0113] (2) Alkali-soluble UV resin, hydroxyethyl methacrylate, photoinitiator 819, epoxy resin KD-242C, aluminum acetylacetonate, additives, and spherical silver powder with an average particle size of 1 μm were mixed at 80° C. and 500 rpm for 4 h to obtain low-temperature sintering.

[0114] 2. The selected substrate is: 96% alumina ceramic, polished to a roughness of less than 1um.

[0115] Screen printing conditions: 360 mesh stainless steel screen printing.

[0116] The drying conditions are: 130°C, 5 minutes.

[0117] The exposure conditions are: 200mj energy, 20um opening film mask.

[0118] The developer conditions are: 0.5% NaHCO3 aqueous solution, and the developing pressure is 0.2 kg.

[0119] The sintering conditions are as follows: debinding at 180°C for 2 hours, heating rate of 10°C / min, keeping at 180°C (low-temperature sintering below 200°C) for 20 minutes, and cooling rate of 10°C / min.

[0120] Test the properties of the cured slurry:

[0121] 1. Resistivity: The resistance value R at both ends of the test line is measured by the milliohm meter.

[0122] 2. Wire diameter: Use a 500x microscope to observe and measure the line width and line spacing (after sintering, the line spacing between each other is 0, which is called no resolution).

[0123] Table 1

[0124] Resistivity (Ω·cm) Line width / μm Line spacing / μm Example 1 <![CDATA[1.5×10 -6 ]]> 23.51 25.04 Example 2 <![CDATA[1.6×10 -6 ]]> 23.78 25.58 Example 3 <![CDATA[1.8×10 -6 ]]> 24.59 26.29 Example 4 <![CDATA[1.9×10 -6 ]]> 24.71 26.31 Comparative Example 1 <![CDATA[4.3×10 -6 ]]> 38.69 42.16 Comparative Example 2 <![CDATA[3.7×10 -6 ]]> No resolution No resolution Comparative Example 3 <![CDATA[3.3×10 -6 ]]> No resolution No resolution

[0125] It can be seen from Table 1 that the alkali-soluble resin of the present invention can effectively reduce the sintering temperature and can be sintered at 180° C., which can effectively improve the resistivity and resolution.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing an alkali-soluble UV resin, characterized in that: The following steps are involved: (1) mixing the first monomer, the second monomer, the third monomer, the initiator, and the molecular weight regulator uniformly, adding the mixture to a solvent, and reacting the mixture under a protective atmosphere at a first temperature for 1 to 4 hours, then at a second temperature for 0.5 to 2 hours, and finally at a third temperature for 0.5 to 2 hours to obtain a copolymer solution; (2) mixing the olefinic acid compound, the polymerization inhibitor and the catalyst uniformly, adding the mixture to the copolymer solution, reacting the mixture at 80 to 110° C. in an oxygen atmosphere until the acid value drops below 5 mgKOH / g, thereby obtaining a modified copolymer solution; (3) adding an acid anhydride compound to the modified copolymer solution and reacting at 80 to 120° C. to obtain an alkali-soluble UV resin; The first monomer includes at least one of isobornyl methacrylate, isobornyl acrylate, acryloyl morpholine, and styrene; The second monomer includes at least one of glycidyl methacrylate and glycidyl acrylate; The structural formula of the third monomer is shown in Formula I: In formula I, R1 is hydrogen or methyl; R2 is (CH2) n CH3 or at least one of the following groups: n is an integer from 0 to 18.

2. The method for preparing the alkali-soluble UV resin according to claim 1, characterized in that: The mass ratio of the first monomer, the second monomer, the third monomer, the initiator, the molecular weight regulator and the solvent is (5-15): (15-40): (5-25): (0.5-2): (0.1-1.5): (30-65).

3. The method for preparing the alkali-soluble UV resin according to claim 1, characterized in that: The molecular weight regulator includes at least one of 3-mercaptopropionate, isooctyl ester, tert-dodecyl mercaptan, n-dodecyl mercaptan, secondary dodecyl mercaptan, and mercaptoethanol; The initiator comprises at least one of diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide, di-tert-amyl peroxide, diisopropyl peroxide and di-tert-butyl peroxide.

4. The method for preparing an alkali-soluble UV resin according to claim 1, characterized in that: The solvent includes at least one of isophorone, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ester, propylene glycol methyl ether, trimethylbenzene, and tetramethylbenzene.

5. The method for preparing the alkali-soluble UV resin according to claim 1, characterized in that: The olefinic acid compound includes at least one of 2,6-dimethyl-1,6-heptadiene-4-carboxylic acid, 1,6-heptadiene-4-carboxylic acid, acrylic acid, and methacrylic acid; The polymerization inhibitor is at least one of p-methoxyphenol, 2,6-di-tert-butyl-4-methylphenol, hydroquinone, p-tert-butylcatechol or 2,6-dinitro-p-cresol; The catalyst is at least one of benzyldimethylamine, triphenylphosphine, aluminum acetylacetonate, tetrabutylammonium bromide, tetraethylammonium bromide, benzyltriethylammonium chloride and triethylamine; The acid anhydride compound includes at least one of phthalic anhydride, dodecyl succinic anhydride, methyl nadic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

6. The method for preparing an alkali-soluble UV resin according to claim 1, characterized in that: The mass ratio of the copolymer solution, the olefinic acid compound, the polymerization inhibitor and the catalyst is 100:(8-25):(0.04-2):(0.3-3); The mass ratio of the acid anhydride compound to the modified copolymer solution is (8-20):

100.

7. The method for preparing an alkali-soluble UV resin according to claim 1, characterized in that: The acid anhydride compound includes at least one of phthalic anhydride, dodecyl succinic anhydride, methyl nadic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

8. The method for preparing an alkali-soluble UV resin according to claim 1, characterized in that: The first temperature is T1°C, satisfying: 75°C≤T1≤110°C; The second temperature is T2°C, satisfying 5°C≤T2-T1≤15°C; The third temperature is T3°C, satisfying 10°C≤T3-T2≤15°C.

9. Use of the alkali-soluble UV resin according to any one of claims 1 to 8 in the preparation of low-temperature sintering.

10. A low temperature sintering silver paste, characterized in that: It comprises an alkali-soluble UV resin; the mass percentage of the alkali-soluble UV resin in the low-temperature sintering silver paste is 5 to 20%; The alkali-soluble UV resin is the alkali-soluble UV resin according to any one of claims 1 to 8.