Eugenol-based polymer microsphere, preparation method thereof and carbide material

Through the esterification and polymerization reaction of eugenol-based polymer microspheres, combined with preoxidation and carbonization processes, carbide materials with uniform particle size and low density were prepared, which solved the uneven particle size and large density of existing microwave absorbing materials. The problem of narrow absorption bandwidth significantly improves electromagnetic wave absorption performance and reduces the harm to the environment.

CN118930730AActive Publication Date: 2024-11-12OCEAN UNIV OF CHINA +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410973526.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing microwave absorbing materials have problems such as uneven particle size, large density, narrow effective absorption bandwidth and poor corrosion resistance, which are difficult to meet the needs of high-performance microwave absorbing materials.

Method used

Eugenol-based polymer microspheres were prepared by esterification and polymerization reaction, followed by preoxidation and carbonization to obtain a carbide material with excellent electromagnetic wave absorption properties.

Benefits of technology

Carbide materials with uniform particle size, low density and wide effective absorption bandwidth are achieved, which improves the absorption performance of electromagnetic waves, and is simple in process and environmentally friendly, avoiding the disadvantages caused by metal doping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930730A_ABST
    Figure CN118930730A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electromagnetic wave absorbing materials, and provides eugenol-based polymer microspheres, a preparation method thereof and a carbide material. The preparation method comprises the following steps: taking a eugenol compound and acrylic anhydride as raw materials, and obtaining an esterified monomer under the action of a catalyst; then under the action of an initiator, the esterified monomer and a vinyl monomer are synthesized into eugenol-based polymer microspheres with the particle size of 0.8-1.5 microns through a precipitation polymerization mechanism; and then sequentially carrying out pre-oxidation and carbonization on the polymer microspheres to obtain the carbide material with the particle size of 0.4-1.0 mu m. Compared with other synthesis methods, the preparation method disclosed by the invention is simple in preparation mode, easy to operate and relatively friendly to a human body and the environment, the obtained polymer microspheres have the advantages of monodispersity and uniform particle size distribution, and the finally synthesized carbide material shows excellent performance in the field of electromagnetic wave absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a eugenol-based polymer microsphere and a preparation method thereof, and a carbide material. Background Art

[0002] With the rapid development of information technology, the widespread use of electronic products has brought infinite convenience to people's lives, but at the same time, the electromagnetic wave interference and radiation pollution it generates can cause serious harm to the human body. In the military field, it may also cause detection deviations, etc. Therefore, it is necessary to provide a high-performance microwave absorbing material to control radiation pollution. High-performance microwave absorbing materials should have the following advantages: thin coating, light weight, high absorptivity and absorption over a wide band. Existing microwave absorbing materials, namely absorbing materials, can be divided into carbon materials, ceramics, magnetic metals, ferrites, conductive polymers and metal organic framework materials (MOF). Among them, carbon materials have been widely used in absorbing materials and supercapacitors due to their chemical stability, adjustable dielectric properties, low density, good compatibility and easy combination with other materials.

[0003] Carbon material absorbers include carbon microspheres, carbon fibers, carbon nanotubes, etc. Compared with other absorbers, carbon microspheres have the advantages of good conductivity, large specific surface area, low density, regular morphology, controllable particle size, and controllable elements in carbon microspheres. They can be used alone or as a precursor in combination with other materials. However, the current method of preparing polymer microspheres faces problems such as uneven particle size of polymer microspheres and difficulty in controlling particle size. In addition, current absorbing materials have the disadvantages of high density, narrow effective absorption bandwidth, and poor corrosion resistance. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a eugenol-based polymer microsphere and a preparation method thereof as well as a carbide material.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing eugenol-based polymer microspheres, comprising the following steps:

[0007] (1) mixing a eugenol-based compound, acrylic anhydride and a catalyst to carry out an esterification reaction to obtain an esterification monomer;

[0008] (2) Mixing the esterification monomer, the vinyl monomer, the initiator and the ethanol solution, and performing a polymerization reaction to obtain the eugenol-based polymer microspheres.

[0009] Preferably, the eugenol-based compound in step (1) is eugenol, guaiacol, isoeugenol, o-vanillin or 2,6-dimethoxyphenol; the catalyst is p-toluenesulfonic acid, hydrochloric acid solution, sulfuric acid solution, phosphoric acid, formic acid, metaphosphoric acid or thionyl chloride;

[0010] The mass fraction of the hydrochloric acid solution is 36-38%, and the mass fraction of the sulfuric acid solution is 96-98%.

[0011] Preferably, in step (1), the molar ratio of the eugenol-based compound, acrylic anhydride and catalyst is 1:1-2:0.01-0.04;

[0012] The temperature of the esterification reaction is 35-50° C., and the time of the esterification reaction is 18-36 hours.

[0013] Preferably, the vinyl monomer in step (2) is acrylonitrile, styrene, ethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, N-vinyl pyrrolidone or divinylbenzene; the initiator is azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, ammonium persulfate or potassium persulfate;

[0014] The volume fraction of the ethanol solution is 30-100%.

[0015] Preferably, in step (2), the molar ratio of the esterification monomer to the vinyl monomer is 1-10:1-9; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the initiator is 100:1-2; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the ethanol solution is 3-5:100;

[0016] The polymerization reaction temperature is 70-90° C., and the polymerization reaction time is 2-5 hours.

[0017] The present invention also provides eugenol-based polymer microspheres prepared by the preparation method of the eugenol-based polymer microspheres.

[0018] The present invention also provides a method for preparing a carbide material, comprising the following steps:

[0019] (a) pre-oxidizing eugenol-based polymer microspheres to obtain a pre-oxidized product;

[0020] (b) carbonizing the pre-oxidation product under a protective atmosphere to obtain the carbide material.

[0021] Preferably, the heating rate of the pre-oxidation in step (a) is 1 to 5°C / min, the target temperature of the pre-oxidation is 250 to 400°C, and the holding time of the pre-oxidation is 1 to 2h;

[0022] The heating rate of the carbonization in step (b) is 1 to 5°C / min, the target temperature of the carbonization is 600 to 1000°C, and the holding time of the carbonization is 1 to 3h.

[0023] The present invention also provides the carbide material prepared by the method for preparing the carbide material.

[0024] The invention also provides application of the carbide material in the field of electromagnetic wave absorption materials.

[0025] The beneficial effects of the present invention are:

[0026] The invention uses eugenol-based compounds and acrylic anhydride as raw materials, and obtains esterification monomers under the action of a catalyst; then, the esterification monomers and vinyl monomers are synthesized into eugenol-based polymer microspheres with a particle size of 0.8 to 1.5 μm through a precipitation polymerization mechanism under the action of an initiator; and then, the polymer microspheres are pre-oxidized and carbonized in sequence to obtain a carbide material with a particle size of 0.4 to 1.0 μm. Compared with other synthesis methods, the preparation method of the esterification monomer is simple, easy to operate, and can achieve solvent-free reaction, with a short reaction time, which is more friendly to the human body and the environment; at the same time, the synthesis process of the polymer microspheres is also relatively simple and easy to operate. The ethanol water solvent used is non-toxic and harmless, which reduces the harm to the human body and the environment. The obtained polymer microspheres have the advantages of monodispersity and uniform particle size distribution; compared with traditional carbon materials, the carbide material prepared by the present invention is not doped with metal. As an electromagnetic wave absorber, it can effectively solve the shortcomings of the current magnetic metal absorbing materials with high density, narrow effective absorption bandwidth and poor corrosion resistance. The addition of heteroatoms produces dipole polarization, which can improve the material's absorption performance of electromagnetic waves. The carbide material shows excellent performance in the field of electromagnetic wave absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the esterification monomer in Example 1;

[0028] Figure 2 is the infrared spectrum of the esterified monomer in Example 1 (Wavenumber—wave number, Transmittance—transmittance);

[0029] Figure 3 This is a comparison chart of infrared spectra of the esterified monomer and the eugenol-based polymer microspheres in Example 1 (Wavenumber—wave number, Transmittance—transmittance);

[0030] Figure 4 This is the EDS elemental analysis diagram of the eugenol-based polymer microspheres in Example 1. Figure 4 Among them, (a) is the C element analysis diagram, (b) is the O element analysis diagram, and (c) is the N element analysis diagram;

[0031] Figure 5 The morphology characterization diagrams of the eugenol-based polymer microspheres and the carbide materials in Examples 1 to 4 are shown in FIG. Figure 5 In the figure, (a) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 1, (b) is a morphology characterization diagram of the carbide material in Example 1, (c) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 2, (d) is a morphology characterization diagram of the carbide material in Example 2, (e) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 3, (f) is a morphology characterization diagram of the carbide material in Example 3, (g) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 4, and (h) is a morphology characterization diagram of the carbide material in Example 4;

[0032] Figure 6 The reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of the absorbing material prepared from the carbide material obtained in Example 1;

[0033] Figure 7 The reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of the absorbing material prepared from the carbide material obtained in Example 2;

[0034] Figure 8 The reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of the absorbing material prepared from the carbide material obtained in Example 3;

[0035] Fig. 9 This is a reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of the absorbing material prepared from the carbide material obtained in Example 4. DETAILED DESCRIPTION

[0036] The present invention provides a method for preparing eugenol-based polymer microspheres, comprising the following steps:

[0037] (1) mixing a eugenol-based compound, acrylic anhydride and a catalyst to carry out an esterification reaction to obtain an esterification monomer;

[0038] (2) Mixing the esterification monomer, the vinyl monomer, the initiator and the ethanol solution, and performing a polymerization reaction to obtain the eugenol-based polymer microspheres.

[0039] In the present invention, the eugenol-based compound in step (1) is preferably a phenolic compound containing a eugenol group, more preferably eugenol, guaiacol, isoeugenol, o-vanillin or 2,6-dimethoxyphenol; the catalyst is preferably p-toluenesulfonic acid, hydrochloric acid solution, sulfuric acid solution, phosphoric acid, formic acid, metaphosphoric acid or thionyl chloride.

[0040] In the present invention, the mass fraction of the hydrochloric acid solution is preferably 36-38%, more preferably 36.5-37.5%, more preferably 37%; the mass fraction of the sulfuric acid solution is preferably 96-98%, more preferably 96.5-97.5%, more preferably 97%.

[0041] In the present invention, the molar ratio of the eugenol-based compound, acrylic anhydride and catalyst in step (1) is preferably 1:1-2:0.01-0.04, more preferably 1:1.25-1.75:0.015-0.035, and more preferably 1:1.4-1.5:0.02-0.03. If the amount of acrylic anhydride used is too low, the remaining eugenol-based compound is too much, which makes it difficult to remove the residue during post-treatment. If the amount of acrylic anhydride used is too high, the price of acrylic anhydride is relatively expensive, resulting in waste and more by-products.

[0042] In the present invention, in step (1), no solvent needs to be added during the esterification reaction, that is, the amount of solvent used is 0, which makes the reaction process easier to operate, can reduce side reactions, and is beneficial to reducing pollution to the environment.

[0043] In the present invention, the mixing in step (1) preferably comprises the following steps: stirring the eugenol-based compound and the catalyst uniformly, and then adding acrylic anhydride under stirring to carry out an esterification reaction.

[0044] In the present invention, the stirring temperature is preferably 35-50°C, further preferably 40-45°C, and more preferably 42-43°C; the stirring speed is preferably 700-1000r / min, further preferably 750-900r / min, and more preferably 800-850r / min; if the stirring speed is higher than 1000r / min, the excessively high stirring speed will make the reaction system unstable, resulting in the appearance of by-products in the reaction, and even leading to experimental failure; if the stirring speed is lower than 700r / min, the reaction system will be unevenly mixed, the tumbling degree will be insufficient, the reaction contact will be untimely, and the reaction time will be prolonged.

[0045] In the present invention, the temperature of the esterification reaction is preferably 35-50°C, more preferably 40-45°C, more preferably 42-43°C; the time of the esterification reaction is preferably 18-36h, more preferably 24-32h, more preferably 26-28h.

[0046] In the present invention, after the esterification reaction is completed, the obtained system is washed, allowed to stand and filtered in sequence, and then the obtained yellow-brown solid is dried to obtain the esterification monomer.

[0047] In the present invention, washing comprises washing with sodium bicarbonate solution and washing with water in sequence, wherein the mass fraction of the sodium bicarbonate solution is preferably 3-7%, more preferably 4-6%, and more preferably 5%; the number of washing with sodium bicarbonate solution and washing with water is determined by conventional technical means in the art, and the pH value of the solution after washing is neutral; standing, filtering and drying are completed by conventional technical means in the art; the drying method is preferably natural air drying or freeze drying in a cool place.

[0048] In the present invention, the structural formula of the esterification monomer is In the formula, R 1 H, CH=O or OCH 3 , R 2 H, CH 3 , CH 2 -CH=CH 2 or CH=CH-CH 3 .

[0049] In the present invention, in step (1), the phenolic hydroxyl group in the eugenol-based compound undergoes an esterification reaction with the ester group in acrylic anhydride to synthesize two allyl groups or acrylate groups, which have a branched topological structure and rich bio-based retention, providing a polymerized double bond for the next polymerization reaction.

[0050] In the present invention, the vinyl monomer in step (2) is preferably acrylonitrile, styrene, ethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, N-vinyl pyrrolidone or divinylbenzene; the initiator is preferably azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, ammonium persulfate or potassium persulfate.

[0051] In the present invention, the main role of the vinyl monomer in the preparation of eugenol-based polymer microspheres is to change the structure and chemical properties of the compound. For example, the introduction of acrylonitrile monomer can change the charge distribution of the carbide material by providing N atoms and improve the dielectric loss performance.

[0052] In the present invention, the volume fraction of the ethanol solution is preferably 30 to 100%, more preferably 40 to 90%, and even more preferably 50 to 80%.

[0053] In the present invention, the molar ratio of the esterification monomer and the vinyl monomer in step (2) is preferably 1-10:1-9, more preferably 2-9:2-8, and more preferably 5-6:4-5; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the initiator is preferably 100:1-2, more preferably 100:1.2-1.8, and more preferably 100:1.4-1.5; if the amount of initiator is too small, the polymerization rate is small or even no polymerization is possible; if the amount of initiator is too large, waste is caused; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the ethanol solution is preferably 3-5:100, more preferably 3.5-4.5:100, and more preferably 4:100.

[0054] In the present invention, the polymerization reaction is carried out under stirring conditions, and the stirring speed is preferably 600-900r / min, more preferably 725-850r / min, more preferably 750-800r / min; the polymerization reaction temperature is preferably 70-90°C, more preferably 75-85°C, more preferably 80°C; the polymerization reaction time is preferably 2-5h, more preferably 2.8-4.5h, more preferably 2.4-4h.

[0055] In the present invention, when the stirring speed and the reaction time are within the range, if the polymerization reaction temperature is lower than 70°C, the polymerization reaction is not sufficient, and the obtained microspheres have different sizes. If the polymerization reaction temperature is higher than 90°C, the particle size of the obtained microspheres is uncontrollable. When the reaction temperature and the reaction time are within the range, if the stirring speed is lower than 600r / min, the polymer agglomerates. If the stirring speed is higher than 900r / min, the speed is too high and is not conducive to ball formation. When the stirring speed and the reaction temperature are within the range, if the reaction time is shorter than 2h, the monomer polymerization reaction is insufficient and the yield is low. If the reaction time is longer than 5h, the morphology of the microspheres changes after polymerization.

[0056] In the present invention, after the polymerization reaction is completed, the obtained system is sequentially washed with ethanol and filtered, and then the obtained solid is dried to obtain eugenol-based polymer microspheres; the drying temperature is preferably 40-60°C, more preferably 45-55°C, and more preferably 50°C.

[0057] The present invention also provides eugenol-based polymer microspheres prepared by the preparation method of the eugenol-based polymer microspheres.

[0058] In the present invention, the particle size of the eugenol-based polymer microspheres is 0.8 to 1.5 μm.

[0059] The present invention also provides a method for preparing a carbide material, comprising the following steps:

[0060] (a) pre-oxidizing eugenol-based polymer microspheres to obtain a pre-oxidized product;

[0061] (b) carbonizing the pre-oxidation product under a protective atmosphere to obtain the carbide material.

[0062] In the present invention, the heating rate of the pre-oxidation in step (a) is preferably 1-5°C / min, more preferably 2-4°C / min, and more preferably 3°C / min; the target temperature of the pre-oxidation is preferably 250-400°C, more preferably 300-350°C, and more preferably 320-330°C; the holding time of the pre-oxidation is preferably 1-2h, more preferably 1.2-1.8h, and more preferably 1.5-1.6h.

[0063] In the present invention, after the pre-oxidation in step (a) is completed, natural cooling is performed to obtain a pre-oxidation product; the target temperature for natural cooling is preferably 20 to 30°C, more preferably 22 to 28°C, and more preferably 25 to 26°C.

[0064] In the present invention, the protective atmosphere in step (b) is preferably argon or nitrogen; the heating rate of the carbonization is preferably 1-5°C / min, more preferably 2-4°C / min, more preferably 3°C / min; the target temperature of the carbonization is preferably 600-1000°C, more preferably 700-900°C, more preferably 800-850°C; the holding time of the carbonization is preferably 1-3h, more preferably 1.5-2.5h, more preferably 1.8-2h.

[0065] In the present invention, in step (b), if the heating rate is higher than 5°C / min, the polymer microspheres may collapse or fuse and adhere, or even lose their spherical shape due to the high heating rate; if the heating rate is lower than 1°C / min, the heating time may be too long due to the low heating rate, resulting in a waste of time.

[0066] In the present invention, after the carbonization in step (b) is completed, the material is naturally cooled to obtain a carbide material; the target temperature of the natural cooling is preferably 20 to 30°C, more preferably 22 to 28°C, and more preferably 25 to 26°C.

[0067] In the present invention, the method of first pre-oxidizing at a relatively low temperature of 250-400°C and then carbonizing at a relatively high temperature of 600-1000°C is adopted to slowly carbonize the material and retain the basic structure of the carbon skeleton of the material as much as possible.

[0068] The present invention also provides the carbide material prepared by the method for preparing the carbide material.

[0069] In the present invention, the particle size of the carbide material is 0.4 to 1.0 μm.

[0070] The invention also provides application of the carbide material in the field of electromagnetic wave absorption materials.

[0071] In the present invention, the application method is preferably: mixing carbide material with paraffin to form a specific ring with the required size and specification of the instrument, and the mass ratio of carbide material to paraffin is preferably 1:4-6, more preferably 1:4.5-5.5, and more preferably 1:5.

[0072] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0073] Example 1

[0074] 8.21 g of eugenol and 0.22 g of p-toluenesulfonic acid were placed in a three-necked flask and stirred evenly. Then, 9.45 g of acrylic anhydride was added at a temperature of 40° C. and a stirring rate of 800 r / min. The esterification reaction was carried out at 40° C. for 24 hours. After the reaction was completed, the obtained system was washed with a sodium bicarbonate solution (the mass fraction of the sodium bicarbonate solution was 5%) and washed with water in sequence. After the washing, the pH value of the solution was neutral. Then, the system was allowed to stand and filtered in sequence. The obtained yellow-brown solid was placed in a cool place to dry naturally to obtain an esterification monomer. The esterification monomer was acrylic acid-(4-allyl-2-methoxy)phenol ester, and the structural formula was as follows:

[0075]

[0076] The esterification monomer was analyzed by nuclear magnetic resonance proton spectrum analysis using a nuclear magnetic resonance instrument from Qingdao Institute of Bioenergy and Process Technology, Chinese Academy of Sciences. The nuclear magnetic resonance proton spectrum of the esterification monomer in this embodiment is as follows: Figure 1 As shown. Figure 1 You can get it in 1 H NMR (600MHz, DMSO) δ7.03(d,1H,-Ph-H),6.97(s,1H-Ph-H),6.78(d,1H,-Ph-H),6.50(d,1H,=CH 2 ),6.39(q,1H,=CH),6.12(d,1H,=CH 2 ),5.98(m,1H,=CH),5.10(d,1H,=CH 2 ),5.05(d,1H,=CH 2 ),3.74(s,3H,-CH 3 ),3.38(d,,2H,-CH 2 ).

[0077] The esterification monomer was analyzed and measured using a Fourier transform infrared spectrometer from Bruker, Germany. The infrared spectrum of the esterification monomer in this embodiment is as follows: Figure 2 As shown. Figure 2 It can be obtained that IR (KBr) v: CO: 1147.53, C = C (benzene ring skeleton vibration): 1497.52, 1451.33, 1397.31, C = O (secondary amide I band): 1734.27, CH (saturated C stretching vibration): 2936.51; therefore, the esterification monomer was successfully synthesized through the nuclear magnetic resonance hydrogen spectrum and infrared spectrum.

[0078] Add esterification monomer, acrylonitrile, azobisisobutyronitrile and 70% ethanol solution by volume into a three-necked flask (the molar ratio of esterification monomer to acrylonitrile is 7:3, the mass ratio of the total mass of esterification monomer and acrylonitrile to azobisisobutyronitrile is 100:1.5, and the mass ratio of the total mass of esterification monomer and acrylonitrile to ethanol solution is 4:100), mix well, and carry out polymerization reaction at a temperature of 85°C and a stirring speed of 750r / min for 3h. After the reaction, wash the obtained system with ethanol and filter it in sequence, and finally dry it at 60°C to obtain eugenol-based polymer microspheres.

[0079] The infrared spectra of the esterified monomer (labeled as DXAA) and the eugenol-based polymer microspheres (labeled as P(DXAA-AN)) were compared to obtain the infrared spectra comparison diagram of the esterified monomer and the eugenol-based polymer microspheres in this embodiment, as shown in FIG. Figure 3 shown; from Figure 3 It can be seen that at 2238.23cm -1 The peak at the center is the stretching vibration peak of -CN in acrylonitrile monomer, which proves that binary copolymerization is feasible.

[0080] The eugenol-based polymer microspheres were subjected to EDS elemental analysis to obtain an EDS elemental analysis diagram of the eugenol-based polymer microspheres in this embodiment, as shown in FIG. Figure 4 As shown; Figure 4 In the figure, (a) is the C element analysis diagram, (b) is the O element analysis diagram, and (c) is the N element analysis diagram. Figure 4 It can be seen that the N element exists in the polymer microspheres, indicating that acrylonitrile and the esterification monomer are successfully polymerized.

[0081] The eugenol-based polymer microspheres were placed in a crucible, placed in a tubular furnace, heated to 300°C at a heating rate of 1°C / min, kept warm for 1 hour, and naturally cooled to 25°C to obtain a pre-oxidation product; the pre-oxidation product was placed in a tubular furnace, heated to 700°C at a heating rate of 3°C / min under argon as a protective atmosphere, kept warm for 2 hours, and then naturally cooled to 25°C to obtain a carbide material.

[0082] Example 2

[0083] 8.21 g of eugenol and 0.17 g of p-toluenesulfonic acid were placed in a three-necked flask and stirred evenly. Then, 7.56 g of acrylic anhydride was added at a temperature of 40° C. and a stirring rate of 800 r / min. The esterification reaction was carried out at 40° C. for 24 hours. After the reaction, the obtained system was washed with a sodium bicarbonate solution (the mass fraction of the sodium bicarbonate solution was 5%) and washed with water in sequence. After the washing, the pH value of the solution was neutral. Then, the system was allowed to stand and filtered in sequence. The obtained yellow-brown solid was placed in a cool place to dry naturally to obtain an esterification monomer. The esterification monomer was acrylic acid-(4-allyl-2-methoxy)phenol ester, and the structural formula was as follows:

[0084]

[0085] The hydrogen nuclear magnetic resonance spectrum of the esterification monomer in this example and the infrared spectrum of the esterification monomer in this example are the same as those in Example 1, and it is determined that the esterification monomer is successfully synthesized.

[0086] Add esterification monomer, acrylonitrile, azobisisobutyronitrile and 70% ethanol solution by volume into a three-necked flask (the molar ratio of esterification monomer to acrylonitrile is 6:4, the mass ratio of the total mass of esterification monomer and acrylonitrile to azobisisobutyronitrile is 100:1.5, and the mass ratio of the total mass of esterification monomer and acrylonitrile to ethanol solution is 4:100), mix well, and carry out polymerization reaction at a temperature of 85°C and a stirring speed of 750r / min for 3h. After the reaction, wash the obtained system with ethanol and filter it in sequence, and finally dry it at 60°C to obtain eugenol-based polymer microspheres.

[0087] The infrared spectra of the esterified monomer and eugenol-based polymer microspheres in this example are the same as those in Example 1, proving that binary copolymerization is feasible.

[0088] The EDS elemental analysis chart of the eugenol-based polymer microspheres in this example is the same as that in Example 1, indicating that acrylonitrile and the esterification monomer are successfully polymerized.

[0089] The eugenol-based polymer microspheres were placed in a crucible, placed in a tubular furnace, heated to 300°C at a heating rate of 1°C / min, kept warm for 1 hour, and naturally cooled to 25°C to obtain a pre-oxidation product; the pre-oxidation product was placed in a tubular furnace, heated to 700°C at a heating rate of 3°C / min under argon as a protective atmosphere, kept warm for 2 hours, and then naturally cooled to 25°C to obtain a carbide material.

[0090] Example 3

[0091] 8.21 g of eugenol and 0.32 g of p-toluenesulfonic acid were placed in a three-necked flask and stirred evenly. Then, 7.56 g of acrylic anhydride was added at a temperature of 40° C. and a stirring rate of 800 r / min. The esterification reaction was carried out at 40° C. for 24 hours. After the reaction, the obtained system was washed with a sodium bicarbonate solution (the mass fraction of the sodium bicarbonate solution was 5%) and washed with water in sequence. After the washing, the pH value of the solution was neutral. Then, the system was allowed to stand and filtered in sequence. The obtained yellow-brown solid was placed in a cool place to dry naturally to obtain an esterification monomer. The esterification monomer was acrylic acid-(4-allyl-2-methoxy)phenol ester, and the structural formula was as follows:

[0092]

[0093] The hydrogen nuclear magnetic resonance spectrum of the esterification monomer in this example and the infrared spectrum of the esterification monomer in this example are the same as those in Example 1, and it is determined that the esterification monomer is successfully synthesized.

[0094] Add esterification monomer, acrylonitrile, azobisisobutyronitrile and 70% ethanol solution by volume into a three-necked flask (the molar ratio of esterification monomer to acrylonitrile is 4:6, the mass ratio of the total mass of esterification monomer and acrylonitrile to azobisisobutyronitrile is 100:1.5, and the mass ratio of the total mass of esterification monomer and acrylonitrile to ethanol solution is 4:100), mix well, and carry out polymerization reaction at a temperature of 85°C and a stirring speed of 750r / min for 3h. After the reaction, wash the obtained system with ethanol and filter it in sequence, and finally dry it at 60°C to obtain eugenol-based polymer microspheres.

[0095] The infrared spectra of the esterified monomer and eugenol-based polymer microspheres in this example are the same as those in Example 1, proving that binary copolymerization is feasible.

[0096] The EDS elemental analysis chart of the eugenol-based polymer microspheres in this example is the same as that in Example 1, indicating that acrylonitrile and the esterification monomer are successfully polymerized.

[0097] The eugenol-based polymer microspheres were placed in a crucible, placed in a tubular furnace, heated to 300°C at a heating rate of 1°C / min, kept warm for 1 hour, and naturally cooled to 25°C to obtain a pre-oxidation product; the pre-oxidation product was placed in a tubular furnace, heated to 700°C at a heating rate of 3°C / min under argon as a protective atmosphere, kept warm for 2 hours, and then naturally cooled to 25°C to obtain a carbide material.

[0098] Example 4

[0099] 8.21 g of eugenol and 0.28 g of p-toluenesulfonic acid were placed in a three-necked flask and stirred evenly. Then, 8 g of acrylic anhydride was added at a temperature of 45° C. and a stirring rate of 900 r / min. The esterification reaction was carried out at 45° C. for 24 hours. After the reaction was completed, the obtained system was washed with a sodium bicarbonate solution (the mass fraction of the sodium bicarbonate solution was 5%) and washed with water in sequence. After the washing, the pH value of the solution was neutral. Then, the system was allowed to stand and filtered in sequence. The obtained yellow-brown solid was placed in a cool place to dry naturally to obtain an esterification monomer. The esterification monomer was acrylic acid-(4-allyl-2-methoxy)phenol ester, and the structural formula was as follows:

[0100]

[0101] The hydrogen nuclear magnetic resonance spectrum of the esterification monomer in this example and the infrared spectrum of the esterification monomer in this example are the same as those in Example 1, and it is determined that the esterification monomer is successfully synthesized.

[0102] Add esterification monomer, acrylonitrile, azobisisobutyronitrile and 70% ethanol solution by volume into a three-necked flask (the molar ratio of esterification monomer to acrylonitrile is 3:7, the mass ratio of the total mass of esterification monomer and acrylonitrile to azobisisobutyronitrile is 100:1.5, and the mass ratio of the total mass of esterification monomer and acrylonitrile to ethanol solution is 4:100), mix well, and carry out polymerization reaction at a temperature of 85°C and a stirring speed of 750r / min for 3h. After the reaction, wash the obtained system with ethanol and filter it in sequence, and finally dry it at 60°C to obtain eugenol-based polymer microspheres.

[0103] The infrared spectra of the esterified monomer and eugenol-based polymer microspheres in this example are the same as those in Example 1, proving that binary copolymerization is feasible.

[0104] The EDS elemental analysis chart of the eugenol-based polymer microspheres in this example is the same as that in Example 1, indicating that acrylonitrile and the esterification monomer are successfully polymerized.

[0105] The eugenol-based polymer microspheres were placed in a crucible, placed in a tubular furnace, heated to 300°C at a heating rate of 1°C / min, kept warm for 1 hour, and naturally cooled to 25°C to obtain a pre-oxidation product; the pre-oxidation product was placed in a tubular furnace, heated to 700°C at a heating rate of 3°C / min under argon as a protective atmosphere, kept warm for 2 hours, and then naturally cooled to 25°C to obtain a carbide material.

[0106] The eugenol-based polymer microspheres and carbide materials prepared in Examples 1 to 4 were observed using a SU1000 scanning electron microscope produced by Hitachi, and the morphology characterization diagrams of the eugenol-based polymer microspheres and carbide materials in Examples 1 to 4 were obtained, as shown in FIG. Figure 5 As shown; Figure 5 In the figure, (a) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 1, (b) is a morphology characterization diagram of the carbide material in Example 1, (c) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 2, (d) is a morphology characterization diagram of the carbide material in Example 2, (e) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 3, (f) is a morphology characterization diagram of the carbide material in Example 3, (g) is a morphology characterization diagram of the eugenol-based polymer microspheres in Example 4, and (h) is a morphology characterization diagram of the carbide material in Example 4; from Figure 5 It can be obtained that the particle size of the eugenol-based polymer microspheres obtained in Example 1 is 0.87 μm, and the particle size of the carbide material is 0.45 μm; the particle size of the eugenol-based polymer microspheres obtained in Example 2 is 0.98 μm, and the particle size of the carbide material is 0.49 μm; the particle size of the eugenol-based polymer microspheres obtained in Example 3 is 0.80 μm, and the particle size of the carbide material is 0.46 μm; the particle size of the eugenol-based polymer microspheres obtained in Example 4 is 1.0 μm, and the particle size of the carbide material is 0.62 μm.

[0107] The carbide materials and paraffin in Examples 1 to 4 were mixed evenly in a mass ratio of 1:5 to form a coaxial ring shape with an inner diameter of 3.04 mm and an outer diameter of 7.00 mm of the required size specifications of the instrument, namely, an absorbing material. The electromagnetic parameters in the frequency range of 2 to 18 GHz were tested by a coaxial method at room temperature using an Agilent N5224A PNA vector network analyzer. According to the document Luo Kong, et al, "Flexible CNTs / CNF-WPU aerogel for smart electromagnetic wave absorbing with tuning effective absorption bandwidth", Carbon, 207, 2023, 13-22, the reflection loss diagram of the absorbing material was calculated by transmission line theory, and the reflection loss diagram of the absorbing material prepared from the carbide material obtained in Example 1 was obtained, as shown in FIG. Figure 6 As shown; the reflection loss diagram of the absorbing material prepared from the carbide material obtained in Example 2 is as follows Figure 7 As shown; the reflection loss diagram of the absorbing material prepared from the carbide material obtained in Example 3, as shown Figure 8 As shown; the reflection loss diagram of the absorbing material prepared from the carbide material obtained in Example 4 is as follows Fig. 9 shown; from Figures 6 to 9It can be obtained that the absorbing material prepared from the carbide material obtained in Example 1 has a minimum reflection loss of -40.89 dB and an effective absorption bandwidth of 4.96 GHz (10.06-15.02 GHz) under the conditions of a matching thickness of 3.00 mm and a frequency of 12.56 GHz; the absorbing material prepared from the carbide material obtained in Example 2 has a minimum reflection loss of -38.12 dB and an effective absorption bandwidth of 3.34 GHz (5.86-9.20 GHz) under the conditions of a matching thickness of 5.00 mm and a frequency of 7.12 GHz. Hz); the absorbing material prepared from the carbide material obtained in Example 3 has a minimum reflection loss of -30.87 dB and an effective absorption bandwidth of 5.16 GHz (10.24-15.40 GHz) under the conditions of a matching thickness of 3.00 mm and a frequency of 12.88 GHz; the absorbing material prepared from the carbide material obtained in Example 4 has a minimum reflection loss of -25.33 dB and an effective absorption bandwidth of 3.90 GHz (5.03-8.93 GHz) under the conditions of a matching thickness of 5.50 mm and a frequency of 7.13 Hz.

[0108] It can be seen from the above embodiments that the present invention uses eugenol-based compounds and acrylic anhydride as raw materials, and obtains esterification monomers under the action of a catalyst; then, the esterification monomers and vinyl monomers are synthesized into eugenol-based polymer microspheres with a particle size of 0.8 to 1.5 μm through a precipitation polymerization mechanism under the action of an initiator; and then the polymer microspheres are pre-oxidized and carbonized in sequence to obtain a carbide material with a particle size of 0.4 to 1.0 μm. Compared with other synthesis methods, the preparation method of the esterification monomer is simple, easy to operate, and can achieve solvent-free reaction, with a short reaction time, which is more friendly to the human body and the environment; at the same time, the synthesis process of the polymer microspheres is also relatively simple and easy to operate. The ethanol water solvent used is non-toxic and harmless, which reduces the harm to the human body and the environment. The obtained polymer microspheres have the advantages of monodispersity and uniform particle size distribution; compared with traditional carbon materials, the carbide material prepared by the present invention is not doped with metal. As an electromagnetic wave absorber, it can effectively solve the shortcomings of the current magnetic metal absorbing materials with high density, narrow effective absorption bandwidth and poor corrosion resistance. The addition of heteroatoms produces dipole polarization, which can improve the material's absorption performance of electromagnetic waves. The carbide material shows excellent performance in the field of electromagnetic wave absorption.

[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing eugenol-based polymer microspheres, characterized in that: It includes the following steps: (1) mixing a eugenol-based compound, acrylic anhydride and a catalyst to carry out an esterification reaction to obtain an esterification monomer; (2) Mixing the esterification monomer, the vinyl monomer, the initiator and the ethanol solution, and performing a polymerization reaction to obtain the eugenol-based polymer microspheres.

2. The method for preparing eugenol-based polymer microspheres according to claim 1, characterized in that: The eugenol-based compound in step (1) is eugenol, guaiacol, isoeugenol, o-vanillin or 2,6-dimethoxyphenol; the catalyst is p-toluenesulfonic acid, hydrochloric acid solution, sulfuric acid solution, phosphoric acid, formic acid, metaphosphoric acid or thionyl chloride; The mass fraction of the hydrochloric acid solution is 36-38%, and the mass fraction of the sulfuric acid solution is 96-98%.

3. The method for preparing eugenol-based polymer microspheres according to claim 1 or 2, characterized in that: In step (1), the molar ratio of the eugenol compound, acrylic anhydride and catalyst is 1:1-2:0.01-0.04; The temperature of the esterification reaction is 35-50° C., and the time of the esterification reaction is 18-36 hours.

4. The method for preparing eugenol-based polymer microspheres according to claim 3, characterized in that: The vinyl monomer in step (2) is acrylonitrile, styrene, ethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, N-vinyl pyrrolidone or divinylbenzene; the initiator is azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, ammonium persulfate or potassium persulfate; The volume fraction of the ethanol solution is 30-100%.

5. The method for preparing eugenol-based polymer microspheres according to claim 4, characterized in that: In step (2), the molar ratio of the esterification monomer to the vinyl monomer is 1-10:1-9; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the initiator is 100:1-2; the mass ratio of the total mass of the esterification monomer and the vinyl monomer to the ethanol solution is 3-5:100; The polymerization reaction temperature is 70-90° C., and the polymerization reaction time is 2-5 hours.

6. Eugenol-based polymer microspheres prepared by the method for preparing eugenol-based polymer microspheres according to any one of claims 1 to 5.

7. A method for preparing a carbide material, characterized in that: It includes the following steps: (a) pre-oxidizing the eugenol-based polymer microspheres according to claim 6 to obtain a pre-oxidized product; (b) carbonizing the pre-oxidation product under a protective atmosphere to obtain the carbide material.

8. The method for preparing a carbide material according to claim 7, characterized in that: The heating rate of the pre-oxidation in step (a) is 1 to 5°C / min, the target temperature of the pre-oxidation is 250 to 400°C, and the holding time of the pre-oxidation is 1 to 2h; The heating rate of the carbonization in step (b) is 1 to 5°C / min, the target temperature of the carbonization is 600 to 1000°C, and the holding time of the carbonization is 1 to 3h.

9. The carbide material prepared by the method for preparing the carbide material according to claim 7 or 8.

10. Use of the carbide material according to claim 9 in the field of electromagnetic wave absorbing materials.

Citation Information

Patent Citations

  • Method for preparing high-aldehyde content polymer microspheres on basis of lignin

    CN105294957A

  • Acrylonitrile copolymer as well as preparation method and application thereof

    CN116003682A

  • GEMA-MMA copolymer dielectric film as well as preparation method and application thereof

    CN116003846A

  • Eugenol-based special-shaped detachable polymer particle and preparation method thereof

    CN117209660A