Preparation method of high-hydrophilic polymer magnetic microspheres

By grafting hydrophilic groups onto the surface of polymer magnetic microspheres, the problem of unstable hydrophilic modification was solved, and stable hydrophilicity and strong adsorption effect of polymer magnetic microspheres were achieved.

CN118930742APending Publication Date: 2024-11-12SUZHOU KNOWLEDGE & BENEFIT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992804.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing methods for hydrophilic modification of polymer magnetic microspheres are unstable, leading to easy detachment of hydrophilic polymers and strong surface hydrophobicity, resulting in limited adsorption.

Method used

Multiple hydrophilic groups (DEA groups or IDA groups) are grafted onto the surface of polymer magnetic microspheres. These groups react with deionized water, cerium ammonium nitrate solution, and GMA monomer, followed by ammonolysis or IDA reaction, to form stable, strongly hydrophilic polymer magnetic microspheres.

Benefits of technology

The hydrophilicity of the polymer magnetic microspheres was improved, non-specific adsorption was reduced, adsorption was enhanced, and the stability of adsorption was ensured by fixing the site with a magnetic field.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-hydrophilic polymer magnetic microsphere, which comprises the following steps: selecting or preparing a polymer magnetic microsphere with hydroxyl, adding a mixture of the polymer magnetic microsphere with hydroxyl and deionized water into an ammonium ceric nitrate solution in an inert gas environment for primary reaction, adding a GMA (Glycidyl Methacrylate) monomer, stirring for reaction, washing, and drying to obtain the high-hydrophilic polymer magnetic microsphere. The preparation method comprises the following steps: preparing magnetic microspheres of which the surfaces are grafted with GMA, and carrying out ammonolysis reaction on the magnetic microspheres of which the surfaces are grafted with GMA or reacting the magnetic microspheres with IDA to prepare the high-hydrophilic polymer magnetic microspheres. The hydrophilic performance of the surface of the magnetic microsphere can be improved through the hydrophilic groups, non-specific adsorption is reduced, and meanwhile the adsorption effect of the magnetic microsphere can be improved through rich functional groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer microspheres, in particular to a method for preparing highly hydrophilic polymer magnetic microspheres. Background Art

[0002] Polymer magnetic microspheres have a wide range of applications in bioseparation engineering and biomedical engineering, especially in the fields of nucleic acid extraction, cell separation, immobilized enzymes, immunoassays, targeted drugs, and separation and purification of proteins and enzymes.

[0003] In order to improve the hydrophilicity of polymer magnetic microspheres, the surface of polymer magnetic microspheres can be functionalized. For example, hydrophilic polymers can be directly adsorbed on the surface of the microspheres. However, simple physical adsorption leads to unstable interaction between the two. The hydrophilic polymers can easily fall off during use, which is not conducive to application. The surface of polymer magnetic microspheres can also be chemically modified, mainly by sulfonation, nitration, chloromethylation and acylation of the magnetic microspheres. However, the surface hydrophobicity of the microspheres in the above methods is very strong, the adsorption effect is limited, and the adsorption is also unstable. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing highly hydrophilic polymer magnetic microspheres, wherein a plurality of hydrophilic groups (DEA groups or IDA groups, etc.) are grafted on the surface of the polymer magnetic microspheres, and the hydrophilicity of the surface of the polymer magnetic microspheres can be improved by utilizing the hydrophilic groups, and nonspecific adsorption can be reduced. Meanwhile, the abundant functional groups can also improve the adsorption effect. In addition, the polymer magnetic microspheres can be firmly positioned in a magnetic field by means of the magnetic attraction of the polymer magnetic microspheres to ensure the adsorption effect.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing highly hydrophilic polymer magnetic microspheres, comprising the following steps:

[0006] S1) selecting or preparing polymer magnetic microspheres with hydroxyl groups;

[0007] S2) adding cerium ammonium nitrate solution to a mixture of the polymer magnetic microspheres with hydroxyl groups prepared in S1 and deionized water in an inert gas environment for initial reaction, then adding GMA monomer for stirring reaction, washing, and preparing magnetic microspheres with surface grafted GMA;

[0008] S3) The magnetic microspheres with surface grafted GMA prepared in S2 are subjected to aminolysis reaction or reacted with IDA to prepare highly hydrophilic polymer magnetic microspheres.

[0009] As a further optimization, PVA magnetic microspheres were selected as polymer magnetic microspheres with hydroxyl groups in S1.

[0010] As a further optimization, S1 is to prepare polymer magnetic microspheres with hydroxyl groups by subjecting the polymer magnetic microspheres to surface chemical reaction.

[0011] As a further optimization, the polymer magnetic microspheres are one or more of polystyrene magnetic microspheres, PMMA magnetic microspheres or PGMA magnetic microspheres.

[0012] As a further optimization, the initial reaction temperature in S3 is 60-80°C, the reaction time is 0.5-1h, and the stirring reaction time is 6-8h.

[0013] As a further optimization, S3 is a magnetic microsphere with surface grafted GMA, which is subjected to aminolysis reaction to prepare highly hydrophilic polymer magnetic microspheres.

[0014] As a further optimization, S3 is to add diethylamine to the magnetic microspheres with surface grafted GMA to react and prepare highly hydrophilic polymer magnetic microspheres.

[0015] As a further optimization, S3 is to prepare highly hydrophilic polymer magnetic microspheres by reacting the magnetic microspheres with GMA grafted on the surface with IDA.

[0016] As a further optimization, the steps of S3 are:

[0017] S31) adding surface-grafted GMA magnetic microspheres to the sodium salt of IDA;

[0018] S32) adding Na2CO3 solution to adjust the pH value and prepare highly hydrophilic polymer magnetic microspheres.

[0019] As a further optimization, the pH value was 9-11.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] 1. The hydroxyl groups possessed or formed by the polymer magnetic microspheres are used to form multiple hydrophilic groups (DEA groups or IDA groups, etc.) on the surface of the polymer magnetic microspheres through reaction. The hydrophilic groups can improve the hydrophilicity of the surface of the polymer magnetic microspheres, reduce nonspecific adsorption, and the rich functional groups can also improve the adsorption effect;

[0022] 2. In the presence of a magnetic field, polymer magnetic microspheres can quickly move to one side of the magnetic field, thereby enabling rapid separation and ensuring adsorption stability. DETAILED DESCRIPTION

[0023] The following are specific embodiments of the present invention, but the present invention is not limited to these embodiments.

[0024] Example 1

[0025] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0026] S1) preparing polymer magnetic microspheres with hydroxyl groups: the polymer magnetic microspheres are selected from polystyrene magnetic microspheres, 20 g of polystyrene magnetic microspheres and 210 g of ethylene dichloride are weighed, 8 g of chloroacetyl chloride and 4 g of anhydrous aluminum chloride are added, reacted at 30° C. for 24 h, washed with ethanol and deionized water in turn, and dried at 100° C. to prepare magnetic microspheres containing chloroacetyl chloride groups, 10% sodium hydroxide solution is added to 5 g of magnetic microspheres containing chloroacetyl chloride groups, refluxed for 10 h, washed 3 times, and dried to prepare polymer magnetic microspheres with hydroxyl groups;

[0027] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0028] S3) Add 3g IDA and 2g NaOH to 100ml water and mix well, then add 2g magnetic microspheres with surface grafted GMA prepared in S2, adjust the pH value to 10-11 with 2M sodium carbonate solution, react at 60°C for 12h, wash 3 times, and prepare strongly hydrophilic polymer magnetic microspheres, which are surface IDA chelating group microspheres.

[0029] The test showed that the content of bovine hemoglobin adsorbed by it reached 5000mmo / g.

[0030] Example 2

[0031] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0032] S1) preparing polymer magnetic microspheres with hydroxyl groups: the polymer magnetic microspheres are selected from polystyrene magnetic microspheres, 8 g of polystyrene magnetic microspheres and 110 g of ethylene dichloride are weighed, 4.5 g of chloroacetyl chloride and 2 g of anhydrous aluminum chloride are added, reacted at 30° C. for 20 h, washed with ethanol and deionized water in turn, and dried at 100° C. to prepare magnetic microspheres containing chloroacetyl chloride groups, 10% sodium hydroxide solution is added to 5 g of the prepared magnetic microspheres containing chloroacetyl chloride groups, refluxed for 10 h, washed 3 times, and dried to prepare polymer magnetic microspheres with hydroxyl groups;

[0033] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0034] S3) 1 g of the surface-grafted GMA magnetic microspheres prepared in S2 was added to 100 ml of a 50% (V / V) diethylamine aqueous solution, and the mixture was shaken at 80°C for 24 h. The mixture was repeatedly washed with deionized water and then added to ethanolamine, and the mixture was shaken at 40°C for 4 h to prepare strongly hydrophilic polymer magnetic microspheres, which were surface anion exchange group microspheres.

[0035] The test showed that the content of bovine hemoglobin adsorbed by it reached 3000mmol / g.

[0036] Example 3

[0037] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0038] S1) preparing polymer magnetic microspheres with hydroxyl groups: polymer magnetic microspheres are selected from polystyrene magnetic microspheres, 10 g of polystyrene magnetic microspheres and 100 g of dichloroethane are weighed, 4.5 g of chloroacetyl chloride and 2 g of anhydrous aluminum chloride are added, reacted at 30° C. for 24 h, washed with ethanol and deionized water in turn, and dried at 100° C. to prepare magnetic microspheres containing chloroacetyl chloride groups, 20% sodium hydroxide solution is added to 10 g of magnetic microspheres containing chloroacetyl chloride groups prepared in S1, refluxed for 10 h, washed 3 times, and dried to prepare polymer magnetic microspheres with hydroxyl groups;

[0039] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0040] S3) 1 g of the surface-grafted GMA magnetic microspheres prepared in S2 was added to 100 ml of a 50% (V / V) aqueous solution of ethylenediamine, and the mixture was shaken at 70° C. for 24 h. The microspheres were washed three times with deionized water to prepare highly hydrophilic polymer magnetic microspheres, which were surface amino microspheres.

[0041] Conductometric titration showed that the surface amino functional groups were 2000mmol / g, and the adsorbed bovine hemoglobin content reached 3000mmol / g.

[0042] Example 4

[0043] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0044] S1) preparing polymer magnetic microspheres with hydroxyl groups: PGMA magnetic microspheres are selected as the polymer magnetic microspheres, 20 g of PGMA magnetic microspheres are weighed with water and 50 g of 0.5% sulfuric acid, reacted at 50° C. for 8 h, washed with ethanol and deionized water three times in sequence, and dried to prepare polymer magnetic microspheres with hydroxyl groups;

[0045] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0046] S3 added 3g IDA and 2g NaOH to 100ml water and mixed evenly, then added 2g magnetic microspheres with surface grafted GMA prepared by S2, adjusted the pH value to 10-11 with 2M sodium carbonate solution, reacted at 60°C for 12h, washed 3 times, and prepared strongly hydrophilic polymer magnetic microspheres, which were surface IDA chelating group microspheres.

[0047] After testing, the content of bovine hemoglobin adsorbed by it reached 4600mmo / g.

[0048] Example 5

[0049] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0050] S1) preparing polymer magnetic microspheres with hydroxyl groups: PGMA magnetic microspheres are selected as polymer magnetic microspheres, 50 g of PGMA magnetic microspheres are weighed, water and 50 g of 0.5% sulfuric acid are weighed, reacted at 50° C. for 8 h, washed with ethanol and deionized water three times in sequence, and dried to prepare polymer magnetic microspheres with hydroxyl groups;

[0051] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0052] S3 added 3g IDA and 2g NaOH to 100ml water and mixed evenly, then added 2g magnetic microspheres with surface grafted GMA prepared by S2, adjusted the pH value to 10-11 with 2M sodium carbonate solution, reacted at 60°C for 12h, washed 3 times, and prepared strongly hydrophilic polymer magnetic microspheres, which were surface IDA chelating group microspheres.

[0053] The test showed that the content of bovine hemoglobin adsorbed by it reached 6500mmo / g.

[0054] Example 6

[0055] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0056] S1) Preparation of polymer magnetic microspheres with hydroxyl groups: PMMA magnetic microspheres are selected as polymer magnetic microspheres. 20 g of PMMA magnetic microspheres are weighed, washed three times with dimethylformamide (DMF) to remove water, 100 ml of polyethylene glycol (PEG-400) is added, and the temperature is raised to 90-95°C. After 1 hour, about 0.5 g of sodium methoxide is added, and the reaction is continued at this temperature for about 12 hours. After the reaction is completed, the particles are washed several times with methanol and deionized water to obtain surface hydroxylated magnetic PMMA microspheres.

[0057] S2) 5 g of the polymer magnetic microspheres with hydroxyl groups prepared in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C. 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and reacted for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0058] S3 added 3g IDA and 2g NaOH to 100ml water and mixed evenly, then added 2g magnetic microspheres with surface grafted GMA prepared by S2, adjusted the pH value to 10-11 with 2M sodium carbonate solution, reacted at 60°C for 12h, washed 3 times, and prepared strongly hydrophilic polymer magnetic microspheres, which were surface IDA chelating group microspheres.

[0059] The test showed that the content of bovine hemoglobin adsorbed by it reached 5500mmo / g.

[0060] Example 7

[0061] A method for preparing highly hydrophilic polymer magnetic microspheres comprises the following steps:

[0062] S1) selecting the magnetic microspheres with hydroxyl groups as PVA magnetic microspheres;

[0063] S2) 5 g of PVA magnetic microspheres in S1 were added to 100 ml of deionized water, mixed and stirred at 60° C., 10 ml of 0.1 M cerium ammonium nitrate solution (dissolved in 1 M HNO3) was added in an inert gas environment, and 10 ml of glycidyl methacrylate (GMA) was added after 30 minutes, and the reaction was carried out for 6 hours. After the reaction was completed, the product was repeatedly washed with deionized water to prepare magnetic microspheres with surface grafted GMA;

[0064] S3 added 3g IDA and 2g NaOH to 100ml water and mixed evenly, then added 2g magnetic microspheres with surface grafted GMA prepared by S2, adjusted the pH value to 10-11 with 2M sodium carbonate solution, reacted at 60°C for 12h, washed 3 times, and prepared strongly hydrophilic polymer magnetic microspheres, which were surface IDA chelating group microspheres.

[0065] The test showed that the content of bovine hemoglobin adsorbed by it reached 4500mmo / g.

[0066] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for preparing highly hydrophilic polymer magnetic microspheres, characterized in that: The steps include: S1) selecting or preparing polymer magnetic microspheres with hydroxyl groups; S2) adding cerium ammonium nitrate solution to the mixture of polymer magnetic microspheres with hydroxyl groups and deionized water in S1 in an inert gas environment for initial reaction, then adding GMA monomer for stirring reaction, washing, and preparing magnetic microspheres with surface grafted GMA; S3) The magnetic microspheres with surface grafted GMA prepared in S2 are subjected to aminolysis reaction or reacted with IDA to prepare highly hydrophilic polymer magnetic microspheres.

2. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1, characterized in that: In S1, PVA magnetic microspheres are selected as polymer magnetic microspheres with hydroxyl groups.

3. The method for preparing the highly hydrophilic polymer magnetic microspheres according to claim 1, characterized in that: S1 is to prepare polymer magnetic microspheres with hydroxyl groups by subjecting polymer magnetic microspheres to surface chemical reaction.

4. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 3, characterized in that: The polymer magnetic microspheres are one or more of polystyrene magnetic microspheres, PMMA magnetic microspheres or PGMA magnetic microspheres.

5. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1, characterized in that: The initial reaction temperature in S3 is 60-80°C, the reaction time is 0.5-1h, and the stirring reaction time is 6-8h.

6. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1, characterized in that: S3 is a magnetic microsphere with GMA grafted on the surface, which is subjected to aminolysis reaction to prepare highly hydrophilic polymer magnetic microspheres.

7. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1 or 6, characterized in that: S3 is to add diethylamine to the magnetic microspheres with GMA grafted on the surface to react and prepare highly hydrophilic polymer magnetic microspheres.

8. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1, characterized in that: S3 is to prepare highly hydrophilic polymer magnetic microspheres by reacting the magnetic microspheres with GMA grafted on the surface with IDA.

9. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 1 or 8, characterized in that: The steps of S3 are: S31) adding magnetic microspheres with surface grafted GMA to the sodium salt of IDA; S32) adding Na2CO3 solution to adjust the pH value and prepare highly hydrophilic polymer magnetic microspheres.

10. The method for preparing highly hydrophilic polymer magnetic microspheres according to claim 9, characterized in that: The pH value is 9-11.