Acrylate copolymer, pressure-sensitive adhesive, pressure-sensitive adhesive tape and preparation method
By using a combination of acrylate copolymer and tackifying resin in thin adhesive tapes, a network interpenetrating structure is formed, and the problem of insufficient adhesion and durability in the prior art is solved, and high initial adhesion and high adhesion are achieved Force pressure sensitive tape is suitable for high temperature and high humidity environments.
Patent Information
- Application Number
- CN202411020477.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
When pursuing high adhesion and initial adhesion, existing thin adhesive tapes are prone to warping, poor adhesion, and poor durability in high temperature and high humidity environments, and are not easy to rework, resulting in the problem of residual glue.
Using acrylate copolymer as the basis, pressure-sensitive tape with high initial adhesion and adhesion strength is prepared by adding special macromonomers and tackifying resins, and crosslinking agents to form a network interpenetrating structure. .
It has achieved pressure-sensitive tape without residual glue in high temperature and high humidity environments and has good adhesion properties, has good initial adhesion and high adhesion strength, and maintains excellent adhesion effect during long-term use.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pressure-sensitive adhesives, and in particular relates to an acrylate copolymer, a pressure-sensitive adhesive, a pressure-sensitive adhesive tape and a preparation method. Background Art
[0002] In recent years, electronic consumer products, especially mobile phones and tablet computers, have become increasingly thinner and lighter. In order to have sufficient bonding strength, the existing adhesive tapes are generally thicker. This is inconsistent with the thinness and lightness of mobile phones. Therefore, an ultra-thin tape is needed to meet the bonding needs.
[0003] In order to maintain or even improve the adhesive force when the adhesive thickness becomes thinner, a large amount of tackifying resin is added in the prior art. However, adding a large amount of tackifying resin will make the colloid hard, reduce the initial adhesion, and easily cause warping or poor adhesion when laminating materials; while if the initial adhesion is pursued, the colloid is softened or a tackifying resin with a low softening point is added, the colloid cohesion is biased, the durability is poor in a high temperature and high humidity environment after laminating the materials, and it is difficult to rework and is prone to residual glue.
[0004] Therefore, the thin adhesive tape is required to have not only high adhesion performance, but also good initial adhesion and durability in high temperature and high humidity environments. Summary of the invention
[0005] The object of the present invention is to provide an acrylate copolymer, a pressure-sensitive adhesive, a pressure-sensitive tape and a preparation method to solve the above technical problems.
[0006] The first aspect of the present invention provides an acrylate copolymer, comprising the following monomer raw materials in parts by weight:
[0007] 80-96 parts of soft monomer, 2-6 parts of crosslinkable monomer, 1-7 parts of hard monomer, 1-7 parts of special monomer; wherein
[0008] The acrylic acid ester copolymer has a weight average molecular weight of 700,000 to 1,500,000 g / mol and a Tg of -70°C to -30°C.
[0009] In one embodiment of the present application, the soft monomer is one or two of 2-ethylhexyl acrylate, isooctyl (meth)acrylate, butyl acrylate or dodecyl (meth)acrylate;
[0010] The crosslinkable monomer is (meth)acrylic acid or two or more of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl acrylate, and glycidyl (meth)acrylate;
[0011] The hard monomer is one or two of vinyl acetate, isobornyl (meth)acrylate, methyl (meth)acrylate, acrylamide, acryloylmorpholine, and N-vinyl pyrrolidone.
[0012] In one embodiment of the present application, the special monomer is a type of macromolecular monomer with a double bond that can be polymerized with an acrylic ester monomer and has a Tg>80°C, and its molecular weight is between 3000 and 10000; optionally, the special monomer can be a macromolecular monomer containing a vinyl group, an acryl group or a styrene group, specifically, such as AA-6 (synthesized by East Asia of Japan) whose main chain is a methyl methacrylate copolymer, AS-6 (synthesized by East Asia of Japan) whose main chain is a styrene copolymer, and AN-6 (synthesized by East Asia of Japan) whose main chain is a styrene-acrylonitrile copolymer.
[0013] In one embodiment of the present application, the raw material of the acrylic ester copolymer further includes 100 to 200 parts of a solvent;
[0014] The solvent includes one or a combination of multiple of ethyl acetate, toluene, butanone, butyl acetate, and n-hexane.
[0015] In one embodiment of the present application, the raw materials of the acrylic ester copolymer further include:
[0016] 0.68 to 1.5 parts of initiator;
[0017] 0.0 to 0.2 parts of chain transfer agent.
[0018] In one embodiment of the present application, the initiator is one of azobisisobutyronitrile, dibenzoyl peroxide, and azobisisoheptylonitrile;
[0019] The chain transfer agent is one of 2-mercaptoethanol, α-thioglycerol, octyl mercaptan, n-dodecyl mercaptan and tert-dodecyl mercaptan; the chain transfer agent can adjust the molecular weight of the polymer during the polymerization process.
[0020] A second aspect of the present invention provides a method for preparing the acrylic acid ester copolymer as described above, comprising:
[0021] Add all the monomer raw materials into a reaction kettle equipped with a reflux device, nitrogen, a thermometer and a stirring device;
[0022] Add 1 / 2 to 3 / 4 of the solvent, raise the temperature to 64 to 66°C, and pass nitrogen for 60 minutes;
[0023] Add 0.08-0.3 parts of initiator and 0.0-0.2 parts of chain transfer agent and react for 3 hours;
[0024] Add 0.2-0.4 parts of initiator, raise the temperature to 70°C, and continue the reaction for 2 hours;
[0025] Add 0.4 to 0.8 parts of initiator, further raise the temperature to reflux temperature, and cool to room temperature after 5 hours;
[0026] The remaining solvent is added to obtain an acrylic ester copolymer having a solid content of 35 to 45 wt%.
[0027] The third aspect of the present invention provides a pressure-sensitive adhesive comprising the following raw materials in parts by weight:
[0028] 100 parts of the acrylic acid ester copolymer described above;
[0029] 10-50 parts of tackifying resin;
[0030] 0 to 5 parts of a cross-linking agent; wherein
[0031] Adding a tackifying resin can improve the adhesion of the pressure-sensitive adhesive; the tackifying resin is one or more of rosin resin, petroleum resin, terpene resin, terpene phenol resin, and polyketone resin; the softening point of the tackifying resin is preferably 50 to 170° C., more preferably 75 to 160° C.;
[0032] The cross-linked pressure-sensitive adhesive layer is easy to obtain good re-peeling performance; the cross-linking structure can be formed by adding a cross-linking agent to the acrylate copolymer; the cross-linking agent can be one or more combinations of commonly used cross-linking agents such as epoxy cross-linking agents, isocyanate cross-linking agents, aziridine cross-linking agents, metal chelate cross-linking agents, etc.; when the adhesive uses a cross-linking agent, in order to form a cross-linking structure, a cross-linking agent with thermal cross-linking is preferably used, the cross-linking temperature is preferably 30 to 150°C, and the cross-linking time depends on the type of different cross-linking agents, usually 5 minutes to 3 days.
[0033] A third aspect of the present invention provides a method for preparing a pressure-sensitive adhesive tape, comprising:
[0034] Mixing the acrylic copolymer, the tackifying resin and the cross-linking agent and allowing the mixture to stand for degassing;
[0035] Use a coating shaft to coat it on a 12 μm thick polyester film;
[0036] The adhesive film is baked at 40-130° C. for 5-10 minutes to obtain a film with a thickness of 7 μm, which is then laminated with a release film and placed at 40-80° C. for 1-5 days to obtain the pressure-sensitive adhesive tape.
[0037] A fourth aspect of the present invention provides a pressure-sensitive adhesive tape prepared by the method for preparing a pressure-sensitive adhesive tape as described above.
[0038] The beneficial effects of the present invention are that the special macromolecular monomer added to the acrylate copolymer of the present invention has good interfacial adhesion and wettability, especially under high temperature conditions, its adhesion effect is still excellent; and the molecular weight of the acrylate copolymer of the present invention is above 700,000 g / mol, and the main chain contains at least two curable groups, and a dense network interpenetrating structure can be obtained after cross-linking with a small amount of cross-linking agent. At this time, a suitable tackifying resin is selected and added, so that the adhesive has improved adhesion and cohesion on the basis of having a good initial adhesion effect, so it is easy to obtain a better bonding effect; the pressure-sensitive adhesive tape of the present invention has good initial adhesion and high adhesion in the initial stage, and still has no residual adhesive and good adhesion in long-term use in a hot and humid environment.
[0039] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description.
[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below for detailed description as follows. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The abbreviations of the raw materials such as monomers, initiators, solvents, crosslinking agents, etc. used in this application are shown in Table 1.
[0043] Table 1: Raw materials and their abbreviations
[0044] abbreviation name 2-EHA 2-Ethylhexyl acrylate BA Butyl acrylate AA acrylic acid HEA Hydroxyethyl acrylate Vac Vinyl acetate GMA Glycidyl Methacrylate IBOA Isobornyl acrylate AA-6 Macromonomer (synthesized by East Asia, Japan) AIBN Azobisisobutyronitrile NDM n-dodecanethiol EtA Ethyl acetate MEK Butanone L-75 Isocyanate crosslinker NE-100C Epoxy crosslinker
[0045] Example 1
[0046] In a four-necked flask equipped with mechanical stirring, N2 port, thermometer and condensed water, add 84.5 parts of 2-EHA, 3 parts of AA, 0.5 parts of HEA, 5 parts of IBOA, 2 parts of GMA, 5 parts of AA-6, 0.1 parts of n-dodecyl mercaptan and 100 parts of EtAc, stir well, heat to 65°C, nitrogen flow rate is 0.5L / min, and after passing nitrogen for 60 minutes, add 0.1 parts of AIBN, maintain 65°C and nitrogen environment for reaction for 3 hours, add 0.2 parts of AIBN, heat to 70°C and continue to react for 2 hours, heat to reflux temperature, add 0.5 parts of AIBN and continue to react for 5 hours, then cool to room temperature, add the remaining EtAc to obtain polymer A-1.
[0047] The raw material formulas of Examples 2 to 5 are shown in Table 2. The rest of the preparation process is the same as that of Example 1 and will not be described again here. Polymers A-2 to A-5 are obtained respectively.
[0048] Comparative Example 1
[0049] In a four-necked flask equipped with mechanical stirring, N2 port, thermometer and condensed water, add 84.5 parts of 2-EHA, 3 parts of AA, 0.5 parts of HEA, 12 parts of IBOA and 100 parts of EtAc, stir well, heat to 65°C, nitrogen flow rate is 0.5L / min, and after passing nitrogen for 60 minutes, add 0.1 parts of AIBN, maintain 65°C and nitrogen environment for reaction for 3 hours, add 0.2 parts of AIBN, heat to 70°C and continue to react for 2 hours, heat to reflux temperature, add 0.5 parts of AIBN and continue to react for 5 hours, then cool to room temperature, add the remaining EtAc to obtain polymer E-1.
[0050] The raw material formula of Comparative Example 2 is shown in Table 2. The rest of the preparation process is the same as that of Comparative Example 1 and will not be described again here to obtain polymer E-2.
[0051] Table 2: Raw material ratio
[0052]
[0053] Preparation of pressure-sensitive adhesive tape: In each embodiment and comparative example, the pressure-sensitive adhesive tape was mixed, coated and cured according to the formulation given in Table 3.
[0054] Specifically, taking Example 1 as an example, the preparation process is as follows:
[0055] Weigh 100 parts of copolymer, 35 parts of tackifying resin, 0.5 parts of L-75 and 0.01 parts of NE-100C, mix them thoroughly, let them stand for defoaming, apply them on 12 μm thick PET using a coating shaft, heat them at 120°C for 5 minutes, and then laminate them with a release film to ensure that the film thickness is 7 μm. Place them at 55°C for 3 days to obtain the product.
[0056] Table 3: Coating formula
[0057] Copolymer Tackifying resin L-75 NE-100C Example 1 A-1 35 0.5 0.01 Example 2 A-2 35 0.5 0.05 Example 3 A-3 35 0.5 0.05 Example 4 A-4 35 1 0.05 Example 5 A-5 35 1 0.05 Comparative Example 1 E-1 35 1 0.05 Comparative Example 2 E-2 35 1 0.05
[0058] The pressure-sensitive adhesive tape prepared above was subjected to physical property tests, and the test results are shown in Table 4. Among them:
[0059] 1. Peel strength test: Determine with reference to GB / T2792-1998 (180° peel strength test method for pressed adhesive tape). Select SUS304 stainless steel plate with specially treated surface as the adherend.
[0060] 2. Adhesion test: The adhesive tape adhesion test is determined according to GB / T4851-2014, and the failure time of the test tape under load is tested.
[0061] 3. Initial adhesion test: The initial adhesion performance test method of the tape is the rolling ball initial adhesion method (J.DOW method), which is determined in accordance with GB / T4852-2002 (pressure-sensitive adhesive tape initial adhesion test method). The test result is expressed by the ball number of the largest steel ball that the pressure-sensitive tape can adhere to.
[0062] Table 4: Physical properties of adhesive sheet
[0063] Peel force / gf Holding force / h Initial adhesion / # Example 1 1360 >72 8 Example 2 1480 >72 7 Example 3 1170 >72 12 Example 4 1400 >72 5 Example 5 1600 >72 9 Comparative Example 1 700 37 5 Comparative Example 2 900 59 3
[0064] It can be seen from Table 4 that by adding special macromolecular monomers and containing at least two or more curable groups on the main chain of the polymer, adding tackifying resins and compounding two or more curing agents, after cross-linking, the adhesive tape not only has excellent cohesive force, but also has good initial adhesion and high peeling force.
[0065] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. An acrylic acid ester copolymer, characterized in that: The monomer raw materials include the following parts by weight: 80-96 parts of soft monomer, 2-6 parts of cross-linkable monomer, 1-7 parts of hard monomer, 1-7 parts of special monomer; in The acrylic acid ester copolymer has a weight average molecular weight of 700,000 to 1,500,000 g / mol and a Tg of -70°C to -30°C.
2. The acrylate copolymer according to claim 1, characterized in that The soft monomer is one or two of 2-ethylhexyl acrylate, isooctyl (meth)acrylate, butyl acrylate or dodecyl (meth)acrylate; The crosslinkable monomer is (meth)acrylic acid or two or more of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl acrylate, and glycidyl (meth)acrylate; The hard monomer is one or two of vinyl acetate, isobornyl (meth)acrylate, methyl (meth)acrylate, acrylamide, acryloylmorpholine, and N-vinyl pyrrolidone.
3. The acrylate copolymer according to claim 1, characterized in that The special monomer is a macromolecular monomer with a double bond and a Tg>80°C, which can be polymerized with an acrylic acid ester monomer and has a molecular weight between 3000 and 10000.
4. The acrylate copolymer according to claim 1, characterized in that The raw materials of the acrylic ester copolymer also include 100 to 200 parts of solvent; The solvent includes one or a combination of multiple of ethyl acetate, toluene, butanone, butyl acetate, and n-hexane.
5. The acrylate copolymer according to claim 1, characterized in that The raw materials of the acrylic ester copolymer also include: 0.68 to 1.5 parts of initiator; 0.0 to 0.2 parts of chain transfer agent.
6. The acrylate copolymer according to claim 5, characterized in that The initiator is one of azobisisobutyronitrile, dibenzoyl peroxide, and azobisisoheptylnitrile; The chain transfer agent is one of 2-mercaptoethanol, α-thioglycerol, octyl mercaptan, n-dodecyl mercaptan and tert-dodecyl mercaptan.
7. A method for preparing an acrylate copolymer according to any one of claims 1 to 6, characterized in that: include: Add all the monomer raw materials into a reaction kettle equipped with a reflux device, nitrogen, a thermometer and a stirring device; Add 1 / 2 to 3 / 4 of the solvent, raise the temperature to 64 to 66°C, and pass nitrogen for 60 minutes; Add 0.08-0.3 parts of initiator and 0.0-0.2 parts of chain transfer agent based on the weight of the monomer raw material, and react for 3 hours; Add 0.2-0.4 parts of initiator, raise the temperature to 70°C, and continue the reaction for 2 hours; Add 0.4 to 0.8 parts of initiator, further raise the temperature to reflux temperature, and cool to room temperature after 5 hours; The remaining solvent is added to obtain an acrylic ester copolymer having a solid content of 35 to 45 wt%.
8. A pressure-sensitive adhesive, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of the acrylate copolymer according to any one of claims 1 to 6; 10-50 parts of tackifying resin; 0 to 5 parts of a cross-linking agent; wherein The tackifying resin is one or more of rosin resin, petroleum resin, terpene resin, terpene phenol resin, and polyketone resin; the softening point of the tackifying resin is 50 to 170°C; The crosslinking agent may be one or more combinations of commonly used crosslinking agents such as epoxy crosslinking agents, isocyanate crosslinking agents, aziridine crosslinking agents, and metal chelate crosslinking agents.
9. A method for preparing a pressure-sensitive adhesive tape, characterized in that: include: Mixing the acrylic copolymer, the tackifying resin and the cross-linking agent and allowing the mixture to stand for degassing; Use a coating shaft to coat it on a 12 μm thick polyester film; The adhesive film is baked at 40-130° C. for 5-10 minutes to obtain a film with a thickness of 7 μm, which is then laminated with a release film and placed at 40-80° C. for 1-5 days to obtain the pressure-sensitive adhesive tape.
10. A pressure-sensitive adhesive tape prepared by the method for preparing a pressure-sensitive adhesive tape according to claim 9.