Polyether-ether-ketone resin with microporous structure and preparation method thereof

By combining chemical foaming and physical foaming methods during the polymerization reaction of polyether ether ketone resin, the problems of uneven gas permeability and limited foaming ratio in polyether ether ketone foaming materials were solved, and micropores were prepared The high-performance foam material with structure achieves the improvement of cell density and foaming ratio and the reduction of material density.

CN118930772AInactive Publication Date: 2024-11-12JILIN ZHONGYAN HIGH PERFORMANCE PLASTIC CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411254263.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation methods for polyether ether ketone foaming materials have problems such as uneven gas permeation, limited foaming ratio, and complex process, making it difficult to prepare high-performance microporous foam materials.

Method used

During the polymerization reaction of polyether ether ketone resin, chemical foaming method and physical foaming method are combined, and the process parameters are controlled to achieve uniform morphology, low density and large-scale cell morphology by adding chemical foaming agents and physical foaming agents. Preparation of high-performance foam materials with bubble ratio.

Benefits of technology

The cell density and foaming ratio are improved, the material density is reduced, and a high-performance polyether ether ketone resin with microporous structure is obtained, filling the gap in domestic high-performance crystalline polyether ether ketone foaming technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930772A_ABST
    Figure CN118930772A_ABST
Patent Text Reader

Abstract

The invention discloses polyether-ether-ketone resin with a microporous structure and a preparation method thereof, and relates to the technical field of high polymer materials. A foaming agent is added in the polymerization reaction process of polyether-ether-ketone resin, and the polymerization reaction process is selected from at least one of a chain initiation stage, a chain growth stage, a chain termination stage and a chain transfer stage. According to the invention, a polymerization process and a foaming process of the polyether-ether-ketone resin are combined, and compared with direct foaming of a polyether-ether-ketone material, the prepared polyether-ether-ketone resin with the microporous structure has the advantages of higher cell density, higher foaming ratio and lower material density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a polyetheretherketone resin with a microporous structure and a preparation method thereof. Background Art

[0002] Polyetheretherketone (PEEK) is a polymer composed of repeating units containing one ketone bond and two ether bonds in the main chain structure. It is a special polymer material. It has physical and chemical properties such as high temperature resistance and chemical corrosion resistance. It is a type of semi-crystalline polymer material that can be used as a high temperature resistant structural material and electrical insulation material. It can be composited with glass fiber or carbon fiber to prepare reinforcement materials. This material has a large number of applications in the aerospace field, medical device field (as artificial bone to repair bone defects) and industrial field. In order to further broaden the application field of polyetheretherketone materials and give full play to its advantages as a special engineering plastic, it is of great significance to develop lightweight polyetheretherketone.

[0003] Polymer foam materials, also known as foam plastics, have many excellent properties such as low density, good impact resistance, high specific strength, excellent thermal insulation, and good sound insulation due to their special porous structure. Therefore, they are widely used in packaging, warmth, sound insulation, transportation, construction, and medical fields, and have become one of the indispensable materials. With the development of high technology, fields with harsh use environments such as national defense, military industry, and aerospace require foam materials with properties such as high temperature resistance, corrosion resistance, and high mechanical strength. Therefore, the development of high-performance foam materials has become an important research direction. The research on polyetheretherketone foam materials not only broadens the application field of polyetheretherketone, but also has important significance in the lightweight, low-carbon and energy-saving aspects of special engineering plastics.

[0004] There are two main methods for preparing polymer foam materials: chemical foaming and physical foaming. Chemical foaming is to add a chemical foaming agent to the polymer so that it decomposes under heat during processing to produce gas and foam, or chemical reactions occur between the raw material components to produce gas, so that the plastic melt is filled with bubbles. Physical foaming is to fill the polymer with saturated inert gas under a certain pressure to make it fully dissolved, and then quickly increase the temperature or reduce the pressure to make the system reach a supersaturated state, and the gas escapes and foams. In addition, there is also a phase inversion method to prepare foam materials, but the phase inversion method is only applicable to soluble polymers, and it is easy to cause residual solvents in the foam material. As early as the early 1980s, Professor NPSuh proposed the concept of microporous foam plastics and applied supercritical technology to the microporous foaming process. In the early 21st century, the preparation of microporous foam plastics by supercritical foaming technology has been successfully commercialized.

[0005] In the preparation of foaming materials, critical or supercritical CO 2Fluids are difficult to use in the polymerization reaction industrial production process and can only be used in the already formed products for secondary processing to obtain foamed materials. The common method is to place polyetheretherketone or its composite material sheet in near-critical or supercritical CO 2 In the fluid, it is swollen and infiltrated at a saturated temperature of 320-360°C and a saturated pressure of 5-30MPa, then quickly unloaded to normal pressure and cooled to room temperature; the above operation is repeated 1-3 times, and finally annealed. The disadvantages of this method are very obvious. First, there are safety hazards caused by high temperature and high pressure; second, the strength of polyetheretherketone material is extremely high, gas penetration is difficult, the permeability is low, and the diffusion of gas in the resin is even more difficult, which leads to more penetration in the part near the outer layer of the plate, less penetration in the center of the plate, and very uneven pores, resulting in serious unevenness in the overall performance of the plate. In order to achieve a higher foaming ratio, multiple operations are required. It can be said that the process is very cumbersome and the effect is not good; finally, the growth and morphology of the pores are limited by the crystal area, and the thickness of the pre-foamed plate can only be less than 15mm. If the thickness is thicker, the gas cannot continue to penetrate inward.

[0006] Chinese patent CN102924743A discloses a method for preparing a crystalline polyetheretherketone foam material, which is mainly prepared by supercritical CO 2 The method uses a physical foaming method to foam polyetheretherketone beads. The foam beads have a single cell size and a maximum foaming ratio of 16 times. Moreover, the foam beads need to be bonded and formed under high-temperature steam. Since the temperature difference between the double melting peaks of the foam beads is narrow, it is difficult to control the subsequent steam compression molding. Therefore, the preparation method has complex equipment, difficult operation, high technical requirements, and is not convenient for industrial application.

[0007] Chinese patent CN102924743A uses crystalline polyetheretherketone as the base resin, uses critical carbon dioxide, and adopts a rapid decompression method to prepare crystalline polyetheretherketone foam. In order to reduce the influence of crystallization on the foaming result, the polyetheretherketone is heated (330-345℃) to a molten state for foaming to obtain polyetheretherketone foam particles with uniform pores and a foaming ratio of 6-17 times. Since the foaming process requires both the polymer to be in a molten state to increase CO 2 Solubility, but also to retain a certain amount of crystals to ensure sufficient melt strength, so the foaming window is relatively narrow, not easy to control; although the linear amorphous polyetheretherketone foaming window is wider, but there are still low melt strength and low foaming ratio disadvantages, and a large amount of crystallization will not only lead to CO 2 The solubility of gas in the polyetheretherketone matrix is ​​reduced, which affects the nucleation density and limits the growth of bubbles. The irregular crystal distribution makes the morphology of polyetheretherketone foam difficult to control.

[0008] Chinese patent CN105367994A discloses a lightweight, wear-resistant micro-foamed polyetheretherketone composite material and its preparation method and application. A high-temperature foaming agent is used to prepare the micro-foamed polyetheretherketone material, but the foaming ratio of the obtained material is too small, and the apparent density of the material is 1.35g / cm 3 above.

[0009] In summary, for the preparation of polyetheretherketone porous foam materials, the existing methods either have limited foaming ratio or complicated processes. In view of this, in order to solve the deficiencies of the prior art, the present invention provides a polyetheretherketone resin with a microporous structure and a preparation method thereof, which overcomes the shortcomings of long gas saturation time, low solubility, and pore growth and morphology being restricted by the crystal region in the process of preparing high-performance crystalline polyetheretherketone foam materials, and has a good research and development prospect. Summary of the invention

[0010] The purpose of the present invention is to provide a polyetheretherketone resin with a microporous structure and a preparation method thereof. By controlling the process parameters, a high-performance foam material with uniform pore morphology, low density and high foaming ratio is prepared, filling the gap in the domestic high-performance crystalline polyetheretherketone foaming technology.

[0011] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:

[0012] On the one hand, the present invention provides a method for preparing a polyetheretherketone resin with a microporous structure, comprising the following steps: adding a foaming agent during the polymerization reaction of the polyetheretherketone resin; the polymerization reaction process is selected from at least one of a chain initiation stage, a chain growth stage, a chain termination stage, and a chain transfer stage.

[0013] Preferably, the preparation method comprises the following steps: adding a chemical foaming agent and a physical foaming agent during the polymerization reaction of the polyetheretherketone resin.

[0014] Further preferably, the preparation method comprises the following steps: during the polymerization reaction of the polyetheretherketone resin, in the chain initiation stage, using a chemical foaming agent for foaming; in the chain growth stage, using a physical foaming agent for foaming.

[0015] More preferably, the preparation method comprises the following steps:

[0016] S1. Add diphenyl sulfone, hydroquinone, 4,4-difluorobenzophenone, sodium carbonate, potassium carbonate and a chemical foaming agent into an autoclave under the condition of continuous nitrogen flow;

[0017] S2, after heating to melt, start stirring, continue heating to 180°C, maintain constant temperature at 180°C for 1 hour, and allow salt formation reaction to occur;

[0018] S3, continue to heat up to the decomposition temperature of the chemical foaming agent, the speed is 80-150r / min, and the duration is 20-60min;

[0019] S4. Continue to raise the temperature to 310°C. At the same time as the temperature starts to rise, close the valve connecting the autoclave to the outside world to seal the autoclave. Add a physical foaming agent until the pressure in the autoclave reaches 2-50MPa. Keep the temperature at 310°C for 1-2 hours, then release the pressure through a pressure reducing device for 1-20s.

[0020] More preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, diisopropyl azodicarboxylate, barium azodicarboxylate, N,N-dinitrosopentamethylenetetramine, p-toluenesulfonylsemicarbazide, 4,4'-oxybis(benzenesulfonylsemicarbazide), and trihydrazinotriazine.

[0021] More preferably, the chemical foaming agent is selected from at least one of barium azodicarboxylate, p-toluenesulfonyl semicarbazide, 4,4'-oxybis(benzenesulfonyl semicarbazide), and trihydrazinotriazine.

[0022] More preferably, the physical foaming agent is selected from at least one of carbon dioxide, helium, neon and argon.

[0023] More preferably, the physical foaming agent is argon.

[0024] More preferably, the mass ratio of the 4,4-difluorobenzophenone to the chemical foaming agent is 100:0.1-12.

[0025] In another aspect, the present invention provides a polyetheretherketone resin having a microporous structure, wherein the polyetheretherketone resin having a microporous structure is prepared according to the above preparation method.

[0026] Preferably, the polyetheretherketone resin having a microporous structure has a melt index of 8-120 g / 10 min, a test temperature of 400° C., and a test load of 5 kg.

[0027] Preferably, the polyetheretherketone resin having a microporous structure has a crystallinity of less than 40%.

[0028] Preferably, the polyetheretherketone resin having a microporous structure has a foaming ratio of 5-30 times.

[0029] Preferably, the polyetheretherketone resin having a microporous structure is a closed-cell structure, and the closed-cell ratio is greater than 90%.

[0030] The beneficial effects of the present invention are:

[0031] (1) The present invention discloses a method for preparing a polyetheretherketone resin with a microporous structure, which combines a polymerization process of the polyetheretherketone resin with a foaming process. Compared with directly foaming the polyetheretherketone material, the polyetheretherketone resin with a microporous structure prepared by the present invention has a larger pore density and foaming ratio and a lower material density.

[0032] (2) The present invention adds a foaming agent during the polymerization reaction of the polyetheretherketone resin, combines the chemical foaming method with the physical foaming method, and foams the polyetheretherketone resin through a two-step method, thereby increasing the pore density and foaming ratio of the polyetheretherketone resin with a microporous structure and reducing the material density of the polyetheretherketone resin with a microporous structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a scanning electron microscope image of the polyetheretherketone material with a microporous structure prepared in Example 1 of the present invention.

[0034] Figure 2 This is a scanning electron microscope image of the polyetheretherketone material with a microporous structure prepared in Example 2 of the present invention.

[0035] Figure 3 This is the infrared transmission spectrum of the polyetheretherketone material with a microporous structure prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is only an exemplary description of the scope of the present invention, and those skilled in the art can make various changes and modifications to the invention of the present invention based on the disclosed content, and they should also fall within the scope of the present invention.

[0037] The present invention is further described below by way of specific examples. The various chemical reagents used in the examples of the present invention are obtained through conventional commercial channels unless otherwise specified. Unless otherwise specified, the contents described below are all weight contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.

[0038] Example 1

[0039] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 50.67g (0.20mol) of barium azodicarboxylate were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stabilized at 180°C, and the temperature was maintained at 180°C for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180°C to 245°C, at which time barium azodicarboxylate began to decompose, the speed was increased to 100r / min, and the temperature was maintained at 245°C for 20-30 minutes, and then the temperature was raised from 245°C to 310°C. At the beginning of the temperature rise, the valve connecting the reactor to the outside was closed to seal the reactor, and argon was passed until the pressure in the reactor reached 5.0MPa. The temperature was maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling. The pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0040] Example 2

[0041] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 68.78g (0.30mol) of p-toluenesulfonyl semicarbazide were added. After the temperature was raised to melting, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stably reached 180°C, and the constant temperature of 180°C was maintained for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180°C to 220°C, at which time p-toluenesulfonyl semicarbazide began to decompose, the speed was increased to 100r / min, and the temperature was maintained at 220°C for 20-30 minutes, and then the temperature was raised from 220°C to 310°C. At the beginning of the temperature rise, the valve connecting the reactor to the outside was closed to seal the reactor, and argon was passed until the pressure in the reactor reached 5.0MPa. The temperature was maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling. The pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0042] Example 3

[0043] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 133.33g (0.30mol) of 4,4'-oxybis (benzenesulfonyl semicarbazide) were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stably reached 180°C, and the constant temperature of 180°C was maintained for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180°C to 215°C, at which time 4,4'-oxybis(benzenesulfonylaminourea) began to decompose, the speed was increased to 120r / min, and the temperature was maintained at 215°C for 20-30 minutes, then the temperature was raised from 215°C to 310°C, and at the same time of the temperature rise, the valve connecting the reactor to the outside was closed, the reactor was sealed, argon was passed until the pressure in the reactor reached 6.0MPa, and the temperature was maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the agitator reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling, and the pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0044] Example 4

[0045] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 85.8g (0.50mol) of trihydrazinotriazine were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stably reached 180°C, and the constant temperature of 180°C was maintained for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180°C to 265°C, at which time trihydrazinotriazine began to decompose, the speed was increased to 120r / min, and the temperature was maintained at 265°C for 20-30 minutes, then the temperature was raised from 265°C to 310°C, and at the same time of the temperature rise, the valve connecting the reactor to the outside was closed to seal the reactor, and argon was passed until the pressure in the reactor reached 6.0MPa, and the temperature was maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling, and the pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0046] Example 5

[0047] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 101.34g (0.40mol) of barium azodicarboxylate were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stabilized at 180°C, and the temperature was maintained at 180°C for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180℃ to 245℃, at which time the chemical foaming agent began to decompose, the speed was increased to 120r / min, and the temperature was maintained at 245℃ for 20-30 minutes, and then the temperature was raised from 245℃ to 310℃. At the beginning of the temperature rise, the valve connecting the reactor to the outside was closed to seal the reactor, and argon was passed until the pressure in the reactor reached 10.0MPa. The temperature was kept at 310℃ for 1-2 hours. When the torque value of the torque sensor of the agitator reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling. The pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150℃ for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0048] Example 6

[0049] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 205.9g (1.20mol) of trihydrazinotriazine were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stabilized at 180°C, and the constant temperature of 180°C was maintained for 1 hour. The generated water and gas were separated by a condenser and a separator. The temperature was raised from 180℃ to 265℃, at which time the chemical foaming agent began to decompose, the speed was increased to 150r / min, and the temperature was maintained at 265℃ for 20-30 minutes, and then the temperature was raised from 265℃ to 310℃. At the beginning of the temperature rise, the valve connecting the reactor to the outside was closed to seal the reactor, and argon was passed until the pressure in the reactor reached 12.0MPa. The temperature was maintained at 310℃ for 1-2 hours. When the torque value of the torque sensor of the agitator reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured onto a smooth stainless steel plate for cooling. The pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150℃ for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0050] Example 7

[0051] During the polymerization process to form polyetheretherketone material, only chemical foaming occurs.

[0052] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, 44.2g (0.32mol) of potassium carbonate, and 50.67g (0.20mol) of barium azodicarboxylate were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stably reached 180°C. The temperature was maintained at 180°C for 1 hour, and the generated water and gas were separated by a condenser and a separator. The temperature was raised from 180°C to 245°C, at which time barium azodicarboxylate began to decompose, the speed was increased to 100r / min, and the temperature was maintained at 245°C for 20-30 minutes, then the temperature was raised from 245°C to 310°C, and at the same time of starting the temperature increase, the valve connecting the reactor to the outside was closed to seal the reactor until the pressure in the reactor reached 5.0MPa, and the temperature was maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the agitator reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured out onto a smooth stainless steel plate for cooling, and the pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone 5 times, washed with deionized water 5 times, loaded into a stainless steel tray, and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0053] Example 8

[0054] During the polymerization process of polyetheretherketone material, only physical foaming occurs.

[0055] Into a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen was continuously introduced, and 6984.6g (32mol) of diphenyl sulfone, 880.8g (8.0mol) of hydroquinone, 1745.6g (8.0mol) of 4,4-difluorobenzophenone, 1017.6g (9.6mol) of sodium carbonate, and 44.2g (0.32mol) of potassium carbonate were added. After the temperature was raised to melt, stirring was started at a speed of 80r / min, and the reaction system was heated from room temperature until it stably reached 180°C. The temperature was maintained at 180°C for 1 hour, and the generated water and gas were separated by a condenser and a separator. Raise the temperature from 180℃ to 245℃, increase the speed to 100r / min, when the temperature reaches 245℃, close the valve connecting the reactor to the outside world, make the reactor sealed, pass argon until the pressure in the reactor reaches 5.0MPa, continue to raise the temperature to 310℃, keep constant temperature at 310℃ for 1-2 hours, when the torque value of the torque sensor of the stirrer reaches the target value, open the valve to quickly release the pressure, pour the mixture in the kettle onto a smooth stainless steel plate to cool, and control the pressure release time to 5-10s. Crush the cooled material, wash it with acetone 5 times, wash it with deionized water 5 times, put it into a stainless steel tray and put it into an oven at 150℃ for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0056] Comparative Example 1

[0057] No chemical foaming agent and physical foaming agent are added during the polymerization reaction, and the other processes are the same as those in Example 1. Chemical foaming agent and physical foaming agent are added to the polyetheretherketone material obtained by polymerization for foaming, and the foaming process is the same as that in Example 1.

[0058] In a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen is continuously introduced, 6984.6g (32mol) diphenyl sulfone, 880.8g (8.0mol) hydroquinone, 1745.6g (8.0mol) 4,4-difluorobenzophenone, 1017.6g (9.6mol) sodium carbonate, 44.2g (0.32mol) potassium carbonate are added, and after heating to melting, stirring is turned on, the speed is 80r / min, and the reaction system is heated from room temperature to 180°C when it stabilizes, and the temperature is maintained at 180°C for 1 hour. The generated water and gas are separated through a condenser and a separator. The temperature is raised from 180°C to 310°C, the speed is increased to 100r / min, and the temperature is maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reaches the target value, the valve is opened to quickly release the pressure, and the mixture in the kettle is poured out onto a smooth stainless steel plate for cooling, and the pressure relief time is controlled at 5-10s. The cooled material was crushed, washed with acetone for 5 times, washed with deionized water for 5 times, loaded into a stainless steel tray, and placed in an oven at 150° C. for 8 hours to obtain a polyetheretherketone product.

[0059] The prepared polyetheretherketone product was put into a 6L sealed high-temperature and high-pressure reactor, 50.67g (0.20mol) of barium azodicarboxylate was added, stirring was started, the speed was 30r / min, and the barium azodicarboxylate began to decompose from room temperature. The valve connecting the reactor to the outside was closed to make the reactor sealed, and the constant temperature of 245°C was maintained for 20-30 minutes. At this time, argon was passed until the air pressure in the reactor reached 5.0MPa, and then the temperature was raised from 245°C to 310°C, and the temperature was kept constant at 310°C for 1-2 hours. When the torque value of the torque sensor of the agitator reached the target value, the valve was opened to quickly release the pressure, and the mixture in the reactor was poured out onto a smooth stainless steel plate for cooling. The pressure relief time was controlled at 5-10s. The cooled material was crushed, washed with acetone for 3 times and deionized water for 3 times to remove the decomposition products of barium azodicarboxylate, and the washed material was placed in a stainless steel tray and placed in an oven at 150° C. for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0060] Comparative Example 2

[0061] No chemical foaming agent is added during the polymerization reaction, and the other processes are the same as those in Example 7. A chemical foaming agent is added to the polyetheretherketone material obtained by polymerization for foaming, and the foaming process is the same as that in Example 7.

[0062] In a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen is continuously introduced, 6984.6g (32mol) diphenyl sulfone, 880.8g (8.0mol) hydroquinone, 1745.6g (8.0mol) 4,4-difluorobenzophenone, 1017.6g (9.6mol) sodium carbonate, 44.2g (0.32mol) potassium carbonate are added, and after heating to melting, stirring is turned on, the speed is 80r / min, and the reaction system is heated from room temperature to 180°C when it stabilizes, and the temperature is maintained at 180°C for 1 hour. The generated water and gas are separated through a condenser and a separator. The temperature is raised from 180°C to 310°C, the speed is increased to 100r / min, and the temperature is maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reaches the target value, the valve is opened to quickly release the pressure, and the mixture in the kettle is poured out onto a smooth stainless steel plate for cooling, and the pressure relief time is controlled at 5-10s. The cooled material was crushed, washed with acetone for 5 times, washed with deionized water for 5 times, loaded into a stainless steel tray, and placed in an oven at 150° C. for 8 hours to obtain a polyetheretherketone product.

[0063] The obtained polyetheretherketone product is put into a 6L sealed high temperature and high pressure reactor, 50.67g (0.20mol) of barium azodicarboxylate is put into it, stirring is started, the speed is 30r / min, and it is heated from room temperature to 245°C. At this time, the barium azodicarboxylate begins to decompose, the valve connecting the reactor to the outside is closed, the reactor is in a sealed state, and the constant temperature of 245°C is maintained for 20-30 minutes. At this time, the pressure in the reactor reaches 3.0MPa, and then the temperature is raised from 245°C to 310°C, and the constant temperature is maintained at 310°C for 2 hours, the valve is opened to quickly release the pressure, and the mixture in the reactor is poured out onto a smooth stainless steel plate for cooling, and the pressure relief time is controlled at 5-10s. The cooled material is crushed, washed with acetone 3 times, and washed with deionized water 3 times to remove the decomposition products of barium azodicarboxylate, and the washed material is loaded into a stainless steel tray and placed in an oven at 150°C for 8 hours to obtain a foamed polyetheretherketone product with a microporous structure.

[0064] Comparative Example 3

[0065] No physical foaming agent is added during the polymerization reaction, and the other processes are the same as those in Example 8. A physical foaming agent is added to the polyetheretherketone material obtained by polymerization for foaming, and the foaming process is the same as that in Example 8.

[0066] In a 6L sealed high-temperature and high-pressure reactor connected to a water separator, a condenser and a stirrer, nitrogen is continuously introduced, 6984.6g (32mol) diphenyl sulfone, 880.8g (8.0mol) hydroquinone, 1745.6g (8.0mol) 4,4-difluorobenzophenone, 1017.6g (9.6mol) sodium carbonate, 44.2g (0.32mol) potassium carbonate are added, and after heating to melting, stirring is turned on, the speed is 80r / min, and the reaction system is heated from room temperature to 180°C when it stabilizes, and the temperature is maintained at 180°C for 1 hour. The generated water and gas are separated through a condenser and a separator. The temperature is raised from 180°C to 310°C, the speed is increased to 100r / min, and the temperature is maintained at 310°C for 1-2 hours. When the torque value of the torque sensor of the stirrer reaches the target value, the valve is opened to quickly release the pressure, and the mixture in the kettle is poured out onto a smooth stainless steel plate for cooling, and the pressure relief time is controlled at 5-10s. The cooled material was crushed, washed with acetone for 5 times, washed with deionized water for 5 times, loaded into a stainless steel tray, and placed in an oven at 150° C. for 8 hours to obtain a polyetheretherketone product.

[0067] The obtained polyetheretherketone product is put into a 6L sealed high-temperature and high-pressure reactor, and the stirring is turned on at a speed of 30r / min. It is heated from room temperature to 245°C, and the valve connecting the reactor to the outside is closed to make the reactor sealed. The temperature is maintained at 245°C for 20-30 minutes. At this time, argon is passed until the pressure in the reactor reaches 5.0MPa, and then the temperature is raised from 245°C to 310°C. The temperature is kept at 310°C for 2 hours, and the valve is opened to quickly release the pressure. The material in the reactor is poured out onto a smooth stainless steel plate for cooling, and the pressure relief time is controlled at 5-10s. The cooled material is a foamed polyetheretherketone product with a microporous structure.

[0068] Detection Methods

[0069] 1. Melt index

[0070] The test method is based on the method in standard ISO 1133, with a test temperature of 380°C and a load of 5 kg.

[0071] 2. Crystallinity

[0072] The test method refers to standard ISO 11357, using DSC method to test crystallinity, with a heating range of 40-400°C and a heating rate of 10°C / min.

[0073] The heat of fusion (ΔH) was obtained by connecting two points of the melting endotherm that deviated from a relatively straight baseline. m ), the enthalpy of the melting transition (mJ) is obtained by integrating the area under the endothermic peak as a function of time: the mass-normalized heat of fusion (J / g) is calculated by dividing the enthalpy by the mass of the sample. The level of crystallinity (%) is determined by dividing the heat of fusion of the sample by the heat of fusion of a completely crystalline polymer (130 J / g for polyetheretherketone).

[0074] 3. Cell density

[0075] The cross section of the foamed polymer material was analyzed using a scanning electron microscope (SEM) to examine the cell density of the foamed polymer material. The analysis instrument used was a JSM-6460LV scanning electron microscope from JEOL, Japan. The cell density is the number of cells per cubic centimeter of the foamed sample. The cell density is determined according to the Kumar method, which is: count the number of cells n (>100) from the SEM photo, and determine the photo area A (cm 2 ) and magnification M, the calculation formula is: cell density N f =(nM 2 / A) 3 / 2

[0076] 4. Material density

[0077] The test method refers to standard GB T6343-2009.

[0078] 5. Foaming ratio

[0079] The ratio of the volume after foaming to that before foaming is the foaming ratio.

[0080] 6. Closed-cell rate

[0081] The test method refers to standard ISO4590-2016.

[0082] Table 1

[0083]

[0084] Note: The theoretical gas evolution of barium azodicarboxylate is calculated as 170 mL / g; the theoretical gas evolution of 4,4'-oxybis(benzenesulfonylamino urea) is calculated as 145 mL / g; the theoretical gas evolution of trihydrazinotriazine is calculated as 247 mL / g; the theoretical gas evolution of p-toluenesulfonylamino urea is calculated as 140 mL / g.

[0085] Table 2

[0086] Melt index (g / 10min) Crystallinity(%) Foaming ratio Closed cell rate (%) Example 1 10.8 26.8 8.2 92 Example 2 20.6 28.2 9.5 93 Example 3 28.9 28.8 18.6 95 Example 4 56.2 29.1 21.4 92 Example 5 85.7 30.4 14.7 96 Example 6 100.6 32.1 28.9 94 Example 7 10.5 27.2 5.1 93 Example 8 11.0 27.5 6.3 91 Comparative Example 1 10.5 28.1 1.5 32 Comparative Example 2 10.2 27.9 1.1 23 Comparative Example 3 10.6 26.7 1.2 18

[0087] Compared with Comparative Example 1, Example 1 has a larger cell density and expansion ratio, and a lower material density; compared with Comparative Example 2, Example 7 has a larger cell density and expansion ratio, and a lower material density; compared with Comparative Example 3, Example 8 has a larger cell density and expansion ratio, and a lower material density. The above technical effects illustrate that, compared with directly foaming the polyetheretherketone material, the polyetheretherketone resin having a microporous structure prepared by combining the polymerization process of the polyetheretherketone resin with the foaming process has a larger cell density and expansion ratio, and a lower material density.

[0088] Compared with Example 7 and Example 8, Example 1 has greater cell density and expansion ratio, and lower material density. The above technical effects illustrate that by adding chemical foaming agent and physical foaming agent during the polymerization reaction of polyetheretherketone resin, and foaming polyetheretherketone resin by two-step method, the cell density and expansion ratio of polyetheretherketone resin with microporous structure are increased, and the material density of polyetheretherketone resin with microporous structure is reduced.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyetheretherketone resin having a microporous structure, characterized in that: The following steps are involved: A chemical foaming agent and a physical foaming agent are added during the polymerization reaction of the polyetheretherketone resin; the polymerization reaction process is selected from at least one of a chain initiation stage, a chain growth stage, a chain termination stage, and a chain transfer stage.

2. The preparation method according to claim 1, characterized in that: The following steps are involved: During the polymerization process of polyetheretherketone resin, a chemical foaming agent is used for foaming in the chain initiation stage; and a physical foaming agent is used for foaming in the chain growth stage.

3. The preparation method according to claim 2, characterized in that: The following steps are involved: S1. Add diphenyl sulfone, hydroquinone, 4,4-difluorobenzophenone, sodium carbonate, potassium carbonate and a chemical foaming agent into an autoclave under the condition of continuous nitrogen flow; S2, after heating to melt, start stirring, continue heating to 180°C, maintain constant temperature at 180°C for 1 hour, and allow salt formation reaction to occur; S3, continue to heat up to the decomposition temperature of the chemical foaming agent, the speed is 80-150r / min, and the duration is 20-60min; S4. Continue to raise the temperature to 310°C. At the same time as the temperature starts to rise, close the valve connecting the high-pressure reactor to the outside world to make the high-pressure reactor in a sealed state. Add a physical foaming agent until the air pressure in the reactor reaches 2-50MPa. Keep the temperature at 310°C for 1-2 hours, and then release the pressure through a pressure reducing device for 1-20s.

4. The preparation method according to claim 3, characterized in that: The chemical foaming agent is selected from at least one of azodicarbonamide, diisopropyl azodicarboxylate, barium azodicarboxylate, N,N-dinitrosopentamethylenetetramine, p-toluenesulfonylsemicarbazide, 4,4'-oxybis(benzenesulfonylsemicarbazide), and trihydrazinotriazine.

5. The preparation method according to claim 3, characterized in that: The physical foaming agent is selected from at least one of carbon dioxide, helium, neon and argon.

6. The preparation method according to claim 3, characterized in that: The mass ratio of the 4,4-difluorobenzophenone to the chemical foaming agent is 100:0.1-12.

7. A polyetheretherketone resin having a microporous structure, characterized in that: The polyetheretherketone resin with a microporous structure is prepared according to the preparation method according to any one of claims 1 to 6.

8. The polyetheretherketone resin with a microporous structure according to claim 7, characterized in that: The polyetheretherketone resin with a microporous structure has a foaming ratio of 5-30 times.

9. The polyetheretherketone resin having a microporous structure according to claim 7, characterized in that: The polyetheretherketone resin with a microporous structure is a closed-cell structure, and the closed-cell ratio is greater than 90%.

10. The polyetheretherketone resin having a microporous structure according to claim 7, characterized in that: The crystallinity of the polyetheretherketone resin with a microporous structure is less than 40%; the melting index of the polyetheretherketone resin with a microporous structure is 8-120g / 10min.

Citation Information

Patent Citations

  • Method for preparing crystalline polyether-ether-ketone foam material

    CN102924743A

  • Lightweight wear-resistant microcellular-foam polyetheretherketone composite material, preparation method and application

    CN105367994A

  • Diatomite / polyether-ether-ketone composite material and preparation method thereof

    CN104559048A

  • KR20230033492A