Method for synthesizing m-cresol-formaldehyde resin for photoresist

Through the reaction of m-p-cresol/o-ethyl phenol and formaldehyde, combined with oxalic acid and formic acid catalysis, the problem of high content of 2,6-dicresol and o-ethyl phenol in tar intermediate para-cresol is solved, and efficient production of m-p-cresol is achieved Cresol resin, used in photoresist, improves product quality and economic benefits.

CN118930773APending Publication Date: 2024-11-12YANCHENG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172648.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the content of 2,6-dicresol and o-ethylphenol in the m-p-cresol extracted from tar is high, which affects the utilization efficiency of m-p-cresol, especially when producing high content of m-p-cresol. , resulting in poor product quality, affecting the application of m-cresol in the enameled wire paint industry.

Method used

The reaction of m-p-cresol/o-ethyl phenol and formaldehyde is carried out by catalyzing the oxalic acid and formic acid complex to form a low molecular weight m-cresol resin, and the molecular weight distribution is obtained by distilling unreacted cresol ando-ethyl phenol. The narrow and light-colored photoresist resin achieves the efficient utilization of m-p-cresol.

Benefits of technology

This method is simple and easy to use, has good process operation, high safety and significant economic benefits. It can be used in areas without isobutene resources. The produced m-cresol resin has high added value, is suitable for photoresist, and has a uniform molecular weight distribution. Performance is better than traditional methods.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for synthesizing m-cresol-formaldehyde resin for photoresist, and belongs to the field of organic synthesis, and the method specifically comprises the following steps: carrying out reduced pressure rectification on m-cresol and p-cresol with high o-ethyl phenol content in a high-efficiency rectifying tower to remove 2, 6-xylenol and 2, 4 / 2, 5-xylenol to obtain m-cresol / o-ethyl phenol of which the content is greater than or equal to 99%; adding the p-cresol / o-ethyl phenolic resin prepolymer, m-cresol / o-ethyl phenol and a catalyst into the reactor, starting stirring, heating to 80-100 DEG C, adding formaldehyde for reaction, keeping the temperature for 1-2 hours after dripping, sampling and analyzing, determining that the m-cresol content is less than or equal to 0.5% through liquid phase or gel chromatography analysis, if the m-cresol content is less than or equal to 0.5%, the m-cresol content is qualified and does not need to be neutralized, heating to distill out unreacted cresol and o-ethyl phenol, and obtaining the m-cresol / o-ethyl phenol. The distilled water layer is a water solution of a p-cresol / o-ethyl phenol mixture with the concentration of 95% or above, and p-cresol / o-ethyl phenol reacts with formaldehyde to obtain a prepolymer for use; and adding a triethylamine acetate adduct into the phenolic resin after free phenol is evaporated out, and performing decompression dehydration to obtain a m-cresol-formaldehyde resin product which is used as a film material for photoresist.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic synthesis, and specifically relates to a method for synthesizing m-cresol-formaldehyde resin for photoresist. Background Art

[0002] Industrial p-cresol is made of crude phenol from the refining workshop of a coking enterprise. After distillation, phenol, o-cresol, m-cresol, and industrial xylenol are obtained, with m-cresol being one of the products. Industrial p-cresol is a colorless to light red liquid, mainly a mixture of m-cresol and p-cresol, wherein the content of m-cresol is 55-45%, p-cresol is 28-45%, and o-cresol is about 1-10%, and the content of o-ethylphenol is ≤2% (coking p-cresol ≤0.5%). It has the odor of pungent phenol, and the color gradually darkens after being left for a long time or exposed to light. It is miscible with alcohol, benzene, ether, etc., slightly soluble in water, corrosive, toxic, with a specific gravity of 1.03-1.05, and a distillation range (95%) of 190-205°C. The content of p-cresol in high-grade p-cresol is above 99%, of which m-cresol is above 64-58% and p-cresol is about 36-43%.

[0003] At present, due to the relatively high price of crude phenol and the good economic value of extracting crude phenol, many coal-to-gas and lignite production companies are working on extracting crude phenol from phenol-containing coal tar. However, the composition of the crude phenol from tar obtained in this way is too different from the gasified crude phenol extracted from coal gasification phenol ammonia water. The contents of 2,6-dimethylphenol and o-ethylphenol, which have a greater impact on the extraction of o-cresol and m-cresol, are high (5 to 10 times that of gasified phenol), which is not conducive to the production of high-content o-cresol and m-cresol. Moreover, the total amount of dimethylphenol is 3 to 5 times that of gasified crude phenol (among which 2,4 / 2,5-dimethylphenol is 5 to 8 times that of gasified phenol). Therefore, the refining of crude phenol from tar will be different from that of traditional gasified crude phenol and high-temperature crude phenol. The content of o-ethylphenol in the m-cresol produced by crude phenol extracted from medium- and low-temperature coal tar is relatively high, generally accounting for 4-15% of m-cresol. Therefore, it will affect the use of m-cresol in the wire enamel industry and the separation of m-cresol, and directly affect the sales of m-cresol. Therefore, it is necessary to study and develop the application of m-cresol extracted from tar.

[0004] In order to reduce the problem of high content of 2,6-dimethylphenol and o-ethylphenol in industrial p-cresol affecting the utilization efficiency of industrial p-cresol, an application method with simple process and economic benefits is urgently needed. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to reduce the problem that the high content of 2,6-dimethylphenol and o-ethylphenol in industrial m-cresol affects the utilization efficiency of industrial m-cresol. The present invention provides a method for synthesizing m-cresol-aldehyde resin for photoresist. The present invention adopts m-cresol / o-ethylphenol mixture to react with formaldehyde to produce m-cresol-aldehyde resin, which is used on a substrate for photoresist as a special resin.

[0006] The invention utilizes the great difference in the reaction activity of m-cresol, p-cresol, o-ethylphenol and formaldehyde, uses oxalic acid and formic acid complex to catalyze the polymerization of p-cresol / o-ethylphenol to produce a prepolymer, adds m-cresol / o-ethylphenol to the prepolymer to react with formaldehyde to generate a low-molecular-weight m-cresol-formaldehyde resin, then evaporates free unreacted cresol and o-ethylphenol to obtain a p-cresol / o-ethylphenol mixture aqueous solution, adds a small amount of acid-base amphoteric catalyst to the remaining material after evaporating the free phenol, slowly polymerizes while heating and dehydrating, dehydrates to 190-210°C and keeps the temperature for dehydration for 1-2 hours, and obtains a m-cresol-formaldehyde photoresist resin with a narrow molecular weight distribution, light color and a resolution of less than 0.5 microns, thereby achieving the purpose of extracting and utilizing p-cresol / o-ethylphenol while synthesizing the m-cresol-formaldehyde resin photoresist. This method is simpler and easier than the tert-butylation method, has high added value, better process operability, stronger practicality, better safety, more significant economic benefits, and is more practical in areas without isobutylene resources.

[0007] Technical solution: The present invention discloses a method for synthesizing m-cresol-formaldehyde resin for photoresist, comprising the following steps:

[0008] Step 1, adding crude meta-p-cresol / o-ethylphenol into a distillation tower, and performing distillation at the top of the tower under certain pressure and reflux ratio conditions to obtain high-purity meta-p-cresol / o-ethylphenol;

[0009] Step 2: adding a p-cresol / o-ethylphenol mixture aqueous solution, a catalyst, and paraformaldehyde into a reactor to produce a linear p-cresol / o-ethylphenol novolac resin prepolymer;

[0010] Step 3: Mix the linear p-cresol / o-ethylphenol novolac resin prepolymer, high-purity m-cresol / o-ethylphenol, a catalyst, and paraformaldehyde for reaction, evaporate the unreacted cresol and o-ethylphenol, and record the evaporated material as the p-cresol / o-ethylphenol mixture aqueous solution; then, add an acid-base amphoteric compound and dehydrate to obtain the m-cresol novolac resin for photoresist.

[0011] Furthermore, in step 1, the distillation tower is a high-efficiency distillation tower with a theoretical plate number of 100 to 250, the certain pressure refers to vacuum distillation at -0.05 to -0.098 MPakPa, and the reflux ratio is 10 to 30:1;

[0012] In step 1, the crude meta-cresol / o-ethylphenol contains: 75-99% meta-cresol and 1-20% o-ethylphenol. The crude meta-cresol / o-ethylphenol also contains o-cresol, 2,6-dimethylphenol, 2,4 / 2,5-dimethylphenol, etc. Preferably, the crude meta-cresol / o-ethylphenol contains 85-95% meta-cresol.

[0013] In step 1, in the high-purity m-cresol / o-ethylphenol, the total content of m-cresol and o-ethylphenol is 99-100%, o-cresol ≤0.3%, 2,6-dimethylphenol ≤0.3%, and the total amount of 2,4- and 2,5-dimethylphenol ≤0.4%;

[0014] Preferably, in the high-purity m-cresol / o-ethylphenol: the total content of m-cresol and o-ethylphenol is 99.5-100%, o-cresol ≤0.1%, 2,6-dimethylphenol ≤0.1%, and the total amount of 2,4- and 2,5-dimethylphenol ≤0.1%;

[0015] The distillation yield of the high-purity m-p-cresol / o-ethylphenol is ≥95%.

[0016] Furthermore, the step 2 is specifically as follows:

[0017] Add the p-cresol / o-ethylphenol mixture aqueous solution obtained in the previous step 3 and a catalyst into the reactor, start stirring, heat to 80-100° C., add paraformaldehyde in batches for reaction, the adding time is 1-2 hours, keep warm for 1-4 hours after addition, take samples for analysis, and the p-cresol content is less than 20% by liquid chromatography or gel chromatography analysis, thus obtaining a linear p-cresol / o-ethylphenol novolac resin prepolymer.

[0018] Furthermore, in step 2:

[0019] The amount of the catalyst added is 0.1 to 5% of the total mass of p-cresol and o-ethylphenol in the p-cresol / o-ethylphenol mixture aqueous solution;

[0020] The amount of paraformaldehyde added is: the ratio of the molar amount of formaldehyde in the paraformaldehyde to the total molar amount of p-cresol and o-ethylphenol in the p-cresol / o-ethylphenol mixture aqueous solution is (1-1.5):1.

[0021] Furthermore, in step 2 and step 3, the catalyst is one or two of weak acids such as oxalic acid, formic acid, phosphoric acid, etc. Preferably, the catalyst is a mixture of oxalic acid and formic acid, wherein the weight ratio of oxalic acid to formic acid is (1-3): (0-1), and the preferred ratio is 2:0-1.

[0022] Furthermore, the step three specifically includes the following steps:

[0023] Step 3.1, in a reactor equipped with linear p-cresol / o-ethylphenol phenolic resin prepolymer, add high-purity m-cresol / o-ethylphenol obtained in step 1 and a catalyst, start stirring and fully mix, and heat to 80-100° C. and add paraformaldehyde in batches for reaction, the addition time is 1-6 hours, and the temperature is kept for 1-3 hours after the addition, and sampling is analyzed. The content of m-cresol is less than 0.5% by liquid chromatography or gel chromatography analysis, which is qualified;

[0024] Step 3.2, after passing the test, heating to boiling, distilling out the unreacted cresol and o-ethylphenol, and the distilled water layer is a p-cresol / o-ethylphenol mixture aqueous solution; the p-cresol / o-ethylphenol mixture aqueous solution is a mixture of p-cresol / o-ethylphenol and water with a purity of more than 95%;

[0025] Step 3.3, after the unreacted cresol and o-ethylphenol are evaporated, add an acid-base amphoteric compound to the reaction mass, mix well, and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, the water level of the receiver is observed. After the water level is constant within 20 minutes, the vacuum degree is gradually increased to 0.098MPa, and the temperature is further increased for dehydration. When the material temperature in the reactor reaches 190-210°C and no liquid is distilled out, keep warm for 1-2 hours, stop dehydration, break the vacuum with nitrogen, and discharge the material to a stainless steel material tray while hot under nitrogen protection to obtain a white to light yellow meta-cresol-formaldehyde resin product as a film material for photoresist.

[0026] Furthermore, in step 3.1:

[0027] The mass ratio of linear p-cresol / o-ethylphenol phenolic resin prepolymer to high-purity m-cresol / o-ethylphenol (0.4-0.6) is 1; the amount of catalyst added is 0.5-5% of the mass of high-purity m-cresol / o-ethylphenol;

[0028] The amount of paraformaldehyde added is:

[0029] The ratio of the molar amount of formaldehyde in the paraformaldehyde to the total molar amount of p-cresol and o-ethylphenol in the high-purity m-cresol / o-ethylphenol is 0.5-0.9; and the molar amount of formaldehyde in the paraformaldehyde is 0.7-0.9 times the sum of the total molar amount of p-cresol and o-ethylphenol in the high-purity m-cresol / o-ethylphenol and the total molar amount of p-cresol and o-ethylphenol in the aqueous solution of the p-cresol / o-ethylphenol mixture in step 2.

[0030] Furthermore, in the step 3.3, the amount of the acid-base amphoteric compound added is 0.1-10% of the mass of the high-purity m-p-cresol / o-ethylphenol, and the boiling point of the acid-base amphoteric compound is 150-165° C.;

[0031] The acid-base amphoteric compound is mainly composed of fatty acid and pyridine, piperidine, piperazine, organic amines, etc., and is preferably an acetic acid adduct of triethylamine.

[0032] The acid-base amphoteric compound is triethylamine acetate adduct, and the preparation method is as follows: prepare it according to the weight ratio of triethylamine / glacial acetic acid = 5 / 6-15, add triethylamine dropwise into glacial acetic acid under stirring, control the temperature to be lower than 50°C, and recycle the mixed solvent under reduced pressure after mixing until it is almost dry. The recycled mixed solvent is the triethylamine acetate adduct. The physical property parameters of the mixed solvent are: boiling point of about 150-165°C, density of 1.001-1.007g / ml, and the acidity and alkalinity of the mixed solvent is related to the ratio of triethylamine and acetic acid, which can be from weak alkalinity to weak acidity.

[0033] Furthermore, the p-cresol / o-ethylphenol mixture aqueous solution obtained in step 3.2 is used to prepare the next batch of linear p-cresol / o-ethylphenol novolac resin prepolymer, or the material layer is used to separate p-cresol and o-ethylphenol after stratification.

[0034] Further, after the p-cresol / o-ethylphenol aqueous solution is layered, the material layer is used to separate p-cresol and o-ethylphenol, and the steps are as follows:

[0035] 1) the p-cresol / o-ethylphenol mixture aqueous solution is layered to obtain a material layer, wherein the material layer is a mixture of p-cresol and o-ethylphenol;

[0036] 2) Passing a mixture of p-cresol and o-ethylphenol into a fixed bed reactor preheated to 300-500°C in the presence of hydrogen for reaction, wherein a transposition catalyst is installed in the fixed bed reactor, and the p-cresol content in the material coming out of the fixed bed is controlled to be ≤25% and the o-ethylphenol content is ≤10%. The materials generated by the reaction are cooled and collected in an intermediate storage tank;

[0037] 3) Transfer the material in the intermediate storage tank into the kettle of the distillation tower, and perform vacuum distillation to obtain m-p-cresol and m-p-ethylphenol.

[0038] The m-p-cresol refers to a mixture of m-cresol and p-cresol; the m-p-ethylphenol refers to a mixture of m-ethylphenol and p-ethylphenol.

[0039] Furthermore, in step 3.3, a white to light yellow meta-cresol-formaldehyde resin product is obtained, and ethylene glycol and ethanol are added to form a solution, which is used as a film material for photoresist.

[0040] Beneficial effects:

[0041] (1) The present invention utilizes the difference in the reaction activity of m-cresol, p-cresol, o-ethylphenol and formaldehyde to directly produce high-content, high-priced m-cresol-formaldehyde resin, which is mainly used for photosensitive adhesives and photoresists; unreacted p-cresol / o-ethylphenol is evaporated and all or part of it is used to produce flexible linear phenolic resin prepolymer, so the process is simple, the operation is convenient, and the added value is high, which expands the application range of m-p-cresol / o-ethylphenol.

[0042] (2) The raw materials required for the meta-cresol-formaldehyde resin synthesized by the present invention only need to control the content of 2,4-xylenol and 2,6-xylenol, and the content of p-cresol and o-ethylphenol is not required to be high. The activities of o-ethylphenol and p-cresol in reaction with aldehydes are similar, and the generated meta-cresol-formaldehyde resin forms a straight chain. Therefore, the quality of the meta-cresol-formaldehyde resin produced by partially replacing p-cresol with o-ethylphenol is the same as that of the resin synthesized with pure m-cresol and pure p-cresol (pure m-p-cresol). The quality of the m-cresol-formaldehyde resin mainly depends on the reaction conditions, and the content of p-cresol and o-ethylphenol has little effect on the quality of the m-cresol-formaldehyde resin.

[0043] From the process point of view, the tert-butylation separation of m-cresol requires tert-butylation reaction, distillation separation, acid catalytic de-tert-butylation, neutralization, secondary distillation, etc., which has many steps, high requirements on equipment materials, large investment, and more "three wastes". However, the present invention only needs a few simple steps of resin synthesis, separation of p-cresol / o-ethylphenol, and resin dehydration, with less equipment investment, common equipment, simple and easy-to-control process, less "three wastes", short process separation cycle, large output, and direct acquisition of downstream high value-added products without reduction, so the economic benefits are better than tert-butylation separation.

[0044] (3) The existing process for synthesizing meta-cresol-formaldehyde resin uses pure p-cresol to react with formaldehyde to generate a linear resin prepolymer, and the prepolymer is then reacted with m-cresol and a small amount of formaldehyde to obtain m-cresol-formaldehyde resin. This requires the use of expensive m-cresol and p-cresol, and the added value of the produced resin is not high; the one-step method uses m-p-cresol and formaldehyde to synthesize m-cresol-formaldehyde resin, and the molecular weight of the obtained resin is uneven, with some large and some small, and the molecular weight distribution is wide, and the product performance is poor.

[0045] The invention adopts a two-step method, adopts a unique catalyst to catalyze the resinification reaction, and uses relatively cheap m-p-cresol / o-ethylphenol raw materials, so that the proportion of p-cresol / o-ethylphenol flexible chain segments in the resin chain is controlled and the resin quality is guaranteed, and high-content p-cresol / o-ethylphenol can be extracted, and the extracted p-cresol / o-ethylphenol can be directly used to synthesize linear p-cresol / o-ethylphenol phenolic resin prepolymers, and the production cost and economic benefits are significantly better than those of the existing process.

[0046] (4) The preferred acidic catalysts of the present invention are oxalic acid and formic acid. Formic acid can be evaporated, and oxalic acid will decompose into carbon dioxide and water at high temperature. Another catalyst, triethylamine acetate, is an acid-base amphoteric catalyst that can control the molecular weight and molecular weight distribution of the phenolic resin within a relatively ideal range. Since it does not contain inorganic ions, the synthesized m-cresol-formaldehyde resin has very good electrical properties, thermal properties, softening point, resolution, etc.

[0047] (5) The present invention mainly adopts paraformaldehyde and phenol to carry out the synthesis reaction of phenolic resin, and the phenol-containing wastewater and triethylamine acetate composite catalyst produced in the reaction are used in a copy-made manner, so that the three wastes pollution is very small, and it is basically a clean production process.

[0048] (6) The present invention uses a composite acid-base amphoteric catalyst composed of acetic acid or other organic acid and triethylamine or other organic base, such as pyridine acetate, piperidine acetate, tetrahydropyridine acetate, etc. These composite catalysts have a moderate boiling point and can be basically evaporated during the later heating and dehydration of the phenolic resin, and will not affect the performance of the phenolic resin. The present invention preferably uses triethylamine acetate composite acid-base catalyst with low price, excellent performance and moderate boiling point.

[0049] (7) The raw materials of the present invention, high-purity m-cresol / o-ethylphenol, can also be used for the production of common thermosetting and thermoplastic phenolic resins. Since the raw materials of the present invention contain very low levels of 2,6-xylenol and 2,4-xylenol that affect polymerization, there are few oligomers in the produced phenolic resin, and the linear p-cresol and o-ethylphenol segments in the molecular chain are distributed more evenly. Therefore, the molecular weight of the product is uniform and the molecular weight distribution is narrow, so the performance is better than the same type of phenolic resin produced from common cresol, xylenol, small cresol, etc., which are generally available on the market. DETAILED DESCRIPTION

[0050] The technical solution of the present invention is described in detail below, but the protection scope of the present invention is not limited to the embodiments.

[0051] Example 1

[0052] Step 1: add 10 tons of 95.0% crude meta-p-cresol / o-ethylphenol (0.3% o-cresol, 2.2% 2,6-xylenol, 46.4% meta-cresol, 38.8% p-cresol, 9.8% o-ethylphenol, 2.5% 2,4 / 2,5-xylenol) into a distillation tower kettle (theoretical plate number 250) with stainless steel packing, raise the temperature, collect the front fraction o-cresol and 2,6-xylenol under -0.085 MPa and reflux ratio of 10 to 15:1, reflux for 1 hour for every 2 hours of discharging, and when the content of meta-p-cresol / o-ethylphenol is ≥98% when sampling and analysis is performed, increase the reflux ratio to 15 to 15:1. 18:1, collect the middle fraction at the top of the tower; when the sampling and analysis of the content of m-p-cresol / o-ethylphenol at the top of the tower is ≤99%, change the reflux ratio to 18-22:1 and continue distillation to collect 99% m-p-cresol / o-ethylphenol; when the sampling and analysis of the content of m-p-cresol / o-ethylphenol is ≤98%, stop distillation, and collect 9.47 tons of high-purity m-p-cresol / o-ethylphenol with a content of 99.68% (including 40.65% p-cresol, 49.0% m-cresol, 0.12% 2,6-xylenol, 10.03% o-ethylphenol, 0.10% 2,4-xylenol, and 0.09% 2,5-xylenol), and the extraction rate of m-p-cresol / o-ethylphenol is 97.1%.

[0053] Step 2: adding a p-cresol / o-ethylphenol mixture aqueous solution, a catalyst, and paraformaldehyde into a reactor to produce a linear p-cresol / o-ethylphenol novolac resin prepolymer;

[0054] Specifically, 410.1 kg of p-cresol / o-ethylphenol (326.7 kg of p-cresol, 81.9 kg of o-ethylphenol, 1.3 kg of m-cresol, and 0.2 kg of other phenols) and 239.7 kg of distilled water (containing 5 kg of formaldehyde) obtained by dehydration and recovery in the synthesis of the previous batch of m-cresol-formaldehyde resin were added into a 3000 L enamel kettle, stirring was started, and 2.9 kg of oxalic acid (6 kg dissolved in hot water) and 1.4 kg of formic acid catalyst (the amount of catalyst was 1.05% of the mass of p-cresol / o-ethylphenol) were added in sequence; after the feeding was completed, After completion, use pH test paper to determine the pH of the reaction liquid to be 3.5-4.0, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.3Mpa, and gradually add 121kg of paraformaldehyde at 80℃ (slightly vacuum the upper part of the kettle for feeding; the molar ratio of aldehyde to p-cresol / o-ethylphenol is 1.09:1). The addition time is 2 hours, and the temperature is slowly increased after the addition; the heating rate is strictly controlled within 2℃ / min, and the rate is determined to be 1.5℃ / min to avoid heating too fast, which will cause the reaction liquid to bubble out and affect the resin quality.

[0055] The temperature was raised to 95°C, the reaction temperature was controlled at 95-100°C, stabilized at 98°C, kept warm for 3 hours, and samples were taken for analysis. Liquid chromatography analysis showed that 13% of p-cresol was qualified, and p-cresol / o-ethyl phenolic resin prepolymer was obtained. The prepolymer was cooled to 80°C.

[0056] Step 3: Mix the linear p-cresol / o-ethylphenol novolac resin prepolymer, high-purity m-cresol / o-ethylphenol, a catalyst, and paraformaldehyde for reaction, and evaporate the unreacted cresol and o-ethylphenol. The evaporated material is a p-cresol / o-ethylphenol mixture aqueous solution; then, add an acid-base amphoteric compound, and dehydrate to obtain the m-cresol novolac resin for photoresist. The specific steps are as follows:

[0057] Step 3.1, add 947 kg of 99.68% high-purity m-cresol / o-ethylphenol (40.65% p-cresol, 49.0% m-cresol, 0.12% 2,6-xylenol, 10.03% o-ethylphenol, 0.10% 2,4-xylenol, 0.09% 2,5-xylenol), 7 kg of oxalic acid (dissolved in 10 kg hot water), 3.5 kg of formic acid (the catalyst mass is high-purity m-cresol / o-ethylphenol) in step 1 to the 3000 L enamel kettle containing the prepolymer. 1.11% of the mass of p-cresol); after the feeding is completed, open the steam valve to increase the temperature. The steam pressure should not exceed 0.3Mpa. 150kg of paraformaldehyde (the molar ratio of aldehyde to phenol is 0.58:1, and the molar ratio of aldehyde to phenol in the prepolymerization and polymerization steps is 0.73:1) is gradually added to the kettle at 80°C. The addition time is 2 hours, and the temperature is slowly increased after the addition; the heating rate is strictly controlled within 1.5°C / min, and the rate is determined to be 1.0°C / min to avoid excessive heating, which causes the reaction liquid to bubble out.

[0058] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C and stabilized at 98°C. The temperature was kept for 2 hours and samples were taken for analysis. Liquid chromatography analysis showed that 0.31% of m-cresol was qualified.

[0059] Step 3.2, after passing the test, the temperature is raised for distillation, and the distilled water layer is a mixture of p-cresol / o-ethylphenol and water with a purity of more than 95%;

[0060] In the step 3.2, the evaporated water layer is used for the preparation of the next batch of linear p-cresol / o-ethylphenol phenolic resin prepolymer (or the material layer is used for the transposition of p-cresol and o-ethylphenol to produce m-p-cresol and m-p-ethylphenol after stratification), the evaporated gas is condensed in the reflux condenser and enters the water separator, the water in the water separator continuously flows back into the reactor from the upper part of the water separator for application, and the p-cresol / o-ethylphenol deposited in the lower layer of the water separator is collected in the collecting tank.

[0061] Step 3.3, after there is no obvious oil in the condensate, the temperature is raised to 120°C for further dehydration, 18.3kg solution (containing 9.5kg catalyst) containing the recovered acid-base catalyst and 0.5kg triethylamine acetate adduct are added to the reactor material and mixed, the mass dosage of the acid-base catalyst is 1.06% of the high-purity m-p-cresol / o-ethylphenol, the vacuum device is adjusted, and vacuum dehydration is started. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, the water level of the receiver is observed, and the specific water level is constant within 20 minutes. The above collected water and p-cresol / o-ethylphenol are respectively combined;

[0062] The vacuum degree was gradually increased to 0.098 MPa, and the temperature was further increased for dehydration. When the temperature of the material in the kettle reached 190°C and no liquid was distilled out, the mixture was kept warm for 1 hour, the dehydration was stopped, the vacuum was released with nitrogen, and the material was discharged into a stainless steel plate while hot under nitrogen protection. After cooling, it was crushed and bagged to obtain 709.1 kg of m-cresol-formaldehyde resin with a color of off-white to light yellow. The sample was analyzed for Mw8265, dispersity 2.21, and measurement resolution 0.31 μm. The 18.3 kg solution containing triethylamine acetate catalyst collected in this step was applied.

[0063] All the materials distilled out before 120° C. in the synthesis of all the meta-cresol-formaldehyde resins and water (in the synthesis of all the meta-cresol-formaldehyde resins) were combined separately, wherein the materials contained 99.63% meta-cresol / o-ethylphenol 410.1 kg (326.7 kg p-cresol, 81.9 kg o-ethylphenol, 1.3 kg m-cresol, and 0.2 kg other phenols); in addition, 239.7 kg of water (containing 5 kg of formaldehyde) was distilled out and used for the next batch of synthesis of p-cresol / o-ethylphenol prepolymers.

[0064] Example 2

[0065] Step 1: Same as Example 1

[0066] Step 2: adding a p-cresol / o-ethylphenol mixture aqueous solution, a catalyst, and paraformaldehyde into a reactor to produce a linear p-cresol / o-ethylphenol novolac resin prepolymer;

[0067] Specifically, 190 kg of p-cresol / o-ethylphenol (151.4 kg of p-cresol, 37.9 kg of o-ethylphenol, 0.6 kg of m-cresol, and 0.1 kg of other phenols) and 117 kg of distilled water (containing 2.4 kg of formaldehyde) recovered by dehydration in the previous batch of meta-cresol-formaldehyde resin synthesis were added into a 1500 L enamel kettle, stirring was started, and 1.9 kg of oxalic acid (3 kg dissolved in hot water) and 1 kg of formic acid catalyst (the amount of catalyst was 1.52% of the mass of p-cresol / o-ethylphenol) were added in sequence; after the feeding was completed, Use pH test paper to determine the pH of the reaction liquid to be 3.5-4.0. Adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.3Mpa, and gradually add 77kg of paraformaldehyde at 80℃ (slightly vacuum the upper part of the kettle for feeding; the molar ratio of aldehyde to p-cresol / o-ethylphenol is 1.5:1). The addition time is 2 hours, and the temperature is slowly increased after the addition; the heating rate is strictly controlled within 2℃ / min, and the rate is determined to be 1.5℃ / min to avoid heating too quickly, which will cause the reaction liquid to bubble out and affect the resin quality.

[0068] The temperature was raised to 95°C, the reaction temperature was controlled at 95-100°C, stabilized at 98°C, kept warm for 3 hours, and samples were taken for analysis. Liquid chromatography analysis showed that 10.6% of p-cresol was qualified, and p-cresol / o-ethyl phenolic resin prepolymer was obtained. The prepolymer was cooled to 80°C.

[0069] Step 3: Mix the linear p-cresol / o-ethylphenol novolac resin prepolymer, high-purity m-cresol / o-ethylphenol, a catalyst, and paraformaldehyde for reaction, and evaporate the unreacted cresol and o-ethylphenol. The evaporated material is a p-cresol / o-ethylphenol mixture aqueous solution; then, add an acid-base amphoteric compound, and dehydrate to obtain the m-cresol novolac resin for photoresist. The specific steps are as follows:

[0070] Step 3.1, add 473.5 kg of 99.68% high-purity m-p-cresol / o-ethylphenol (40.65% p-cresol, 49.0% m-cresol, 0.12% 2,6-xylenol, 10.03% o-ethylphenol, 0.10% 2,4-xylenol, 0.09% 2,5-xylenol), 3.5 kg of oxalic acid (5 kg dissolved in hot water), 1.8 kg of formic acid (the catalyst mass dosage is After the feeding is completed, open the steam valve to increase the temperature. The steam pressure should not exceed 0.3Mpa. At a kettle temperature of 80°C, gradually add 78kg of paraformaldehyde (the molar ratio of aldehyde to phenol is 0.6:1, and the molar ratio of aldehyde to phenol in the prepolymerization and polymerization steps is 0.85:1). The addition time is 2 hours, and the temperature is slowly increased after the addition. The heating rate is strictly controlled within 1.5°C / min, and the rate is determined to be 1.0°C / min to avoid excessive heating, which causes the reaction liquid to bubble out.

[0071] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C and stabilized at 98°C. The temperature was kept for 2 hours and samples were taken for analysis. Liquid chromatography analysis showed that the m-cresol content was 0.18%, which was qualified.

[0072] Step 3.2, after passing the test, the temperature is raised for distillation, and the distilled material is a mixture of p-cresol / o-ethylphenol and water with a purity of more than 95%;

[0073] In the step 3.2, the evaporated material is used for the preparation of the next batch of linear p-cresol / o-ethylphenol phenolic resin prepolymer, the evaporated gas is condensed in the reflux condenser and enters the water separator, the water in the water separator continuously flows back into the reactor from the upper part of the water separator for application, and the p-cresol / o-ethylphenol deposited in the lower layer of the water separator is collected in the collecting tank.

[0074] Step 3.3, after there is no obvious oil in the condensate, the temperature is raised to 120°C for further dehydration, 10kg solution containing the recovered acid-base catalyst (containing 5.2kg catalyst) and 0.5kg triethylamine acetate adduct are added to the reactor material and mixed (the mass dosage of the acid-base catalyst is 1.20% of the high-purity m-p-cresol / o-ethylphenol), the vacuum device is adjusted, and vacuum dehydration is started. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, the water level of the receiver is observed, and the specific water level is constant within 20 minutes. The water and p-cresol / o-ethylphenol collected by the above distillation and dehydration are respectively combined;

[0075] The vacuum degree was gradually increased to 0.098 MPa, and the temperature was further increased for dehydration. When the temperature of the material in the kettle reached 190°C and no liquid was distilled out, the temperature was kept for 1 hour, the dehydration was stopped, the vacuum was released with nitrogen, and the material was discharged into a stainless steel plate while hot under nitrogen protection, cooled, and then crushed and bagged to obtain 572.6 kg of m-cresol-formaldehyde resin, which was off-white to light yellow in color. The sample was analyzed for Mw8987, dispersity 2.31, and the measurement resolution was 0.34 μm; 10.1 kg (containing 5.6 kg of triethylamine acetate) collected in this step was used as a solution containing triethylamine acetate catalyst.

[0076] All the materials and water distilled before 120° C. in the synthesis of all meta-cresol-formaldehyde resins are combined separately, wherein the materials contain 99.63% meta-cresol / o-ethylphenol 154.9 kg (p-cresol 123.6 kg, o-ethylphenol 30.7 kg, m-cresol 0.5 kg, other phenols 0.1 kg); in addition, 210.7 kg of water (containing 4 kg of formaldehyde) is distilled off and used for the next batch of synthesis of p-cresol / o-ethylphenol prepolymer.

[0077] Step 4: subjecting the p-cresol / o-ethylphenol recovered from the synthesis of the previous batch of m-cresol-formaldehyde resin to a fixed bed catalytic transposition reaction to obtain a mixture mainly composed of m-cresol and m-ethylphenol, and distilling to obtain m-cresol and m-ethylphenol. The specific process is as follows:

[0078] (1) 220 parts of p-cresol / o-ethylphenol (175.3 kg of p-cresol, 43.9 kg of o-ethylphenol, 0.7 kg of m-cresol, and 0.1 kg of other phenols) were preheated to 190°C and then pumped into a fixed bed reactor preheated to 450°C in the presence of hydrogen using a peristaltic metering pump for reaction (molar ratio of hydrogen to p-cresol / o-ethylphenol was 10:1). The fixed bed reactor was filled with a transposition catalyst composed of 70% H-type MCM-41 / ZSM-5 molecular sieve with 20% clay attached and 10% rare earth. The reaction mixture was stirred for 10 hours. The content of p-cresol was 12.84% and that of o-ethylphenol was 0.45% in the material coming out of the fixed bed. The material generated by the reaction was cooled and collected in an intermediate storage tank. After the reaction, 216.6 parts of a m-cresol mixture (including 4.2 parts of phenol, 6.7 parts of o-cresol, 131.5 parts of m-cresol, 27.0 parts of p-cresol, 1.1 parts of o-ethylphenol, 39.7 parts of m-p-ethylphenol, 2.1 parts of xylenol and 4.3 parts of others) were obtained. The transposition rates of p-cresol and o-ethylphenol were 84.6% and 97% respectively.

[0079] (2) The m-p-cresol in the intermediate storage tank is transferred to the bottom of the distillation tower (theoretical plate number 250, the bottom of the tower is pre-loaded with 50 parts of high boiling point solvent), and distilled at -0.085 MPa and a reflux ratio of 15-20 to obtain 16.8 parts of mixed phenol (4.1 parts of phenol, 6.5 parts of o-cresol, 2.8 parts of m-cresol, 0.6 parts of p-cresol, and 2.8 parts of others), 150.1 parts of 99.2% m-p-cresol (0.1 parts of o-cresol, accounting for 0.07%; 123. 6 parts, accounting for 82.34%; p-cresol 25.3 parts, accounting for 16.86%; o-ethylphenol 0.9 parts, accounting for 0.60%; xylenol 0.1 parts, accounting for 0.07%), intermediate distillates 6.6 parts (m-cresol 3.8 parts, p-cresol 0.8 parts, o-ethylphenol 0.1 parts, m-p-ethylphenol 1.2 parts, xylenol 0.7 parts), 96.7%% m-p-ethylphenol 39.4 parts (m-p-ethylphenol 38.1 parts, xylenol 1.2 parts, others 0.1 parts).

[0080] 99.2% of m-p-cresol and 96.7% of m-p-ethylphenol (including 3,5-xylenol, 2,3-xylenol and other xylenols, the content is 99.75%) are sold as products.

[0081] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention.

Claims

1. A method for synthesizing a m-cresol-formaldehyde resin for photoresist, characterized in that: The steps include: Step 1, adding crude meta-p-cresol / o-ethylphenol into a distillation tower, and performing distillation at the top of the tower under certain pressure and reflux ratio conditions to obtain high-purity meta-p-cresol / o-ethylphenol; Step 2: adding a p-cresol / o-ethylphenol mixture aqueous solution, a catalyst, and paraformaldehyde into a reactor to produce a linear p-cresol / o-ethylphenol novolac resin prepolymer; Step 3: Mix the linear p-cresol / o-ethylphenol novolac resin prepolymer, high-purity m-cresol / o-ethylphenol, a catalyst, and paraformaldehyde for reaction, evaporate the unreacted cresol and o-ethylphenol, and record the evaporated material as the p-cresol / o-ethylphenol mixture aqueous solution; then, add an acid-base amphoteric compound and dehydrate to obtain the m-cresol novolac resin for photoresist.

2. The method according to claim 1, characterized in that In step 1, the distillation tower is a high-efficiency distillation tower with a theoretical plate number of 100 to 250, the certain pressure refers to vacuum distillation at -0.05 to -0.095 MPa, and the reflux ratio is 10 to 30:1; In the high-purity m-p-cresol / o-ethylphenol, the total content of m-p-cresol and o-ethylphenol is 99-100%, o-cresol is ≤0.3%, 2,6-xylenol is ≤0.3%, and the total content of 2,4-xylenol and 2,5-xylenol is ≤0.4%.

3. The method according to claim 1, characterized in that The step 2 is specifically as follows: Add the p-cresol / o-ethylphenol mixture aqueous solution obtained in the previous step 3 and a catalyst into the reactor, start stirring, heat to 80-100° C., add paraformaldehyde in batches for reaction, the adding time is 1-2 hours, keep warm for 1-4 hours after addition, take samples for analysis, and the p-cresol content is less than 20% by liquid chromatography or gel chromatography analysis, thus obtaining a linear p-cresol / o-ethylphenol novolac resin prepolymer.

4. The method according to claim 1, characterized in that: In the step 2, the amount of the catalyst added is 0.1 to 5% of the total mass of p-cresol and o-ethylphenol in the p-cresol / o-ethylphenol mixture aqueous solution; The amount of paraformaldehyde added is: the ratio of the molar amount of formaldehyde in the paraformaldehyde to the total molar amount of p-cresol and o-ethylphenol in the p-cresol / o-ethylphenol mixture aqueous solution is (1-1.5):

1.

5. The method according to claim 1, characterized in that The catalysts in step 2 and step 3 are one or two of oxalic acid, formic acid and phosphoric acid.

6. The method according to claim 5, characterized in that The catalyst is a mixture of oxalic acid and formic acid, wherein the weight ratio of oxalic acid to formic acid is (1-3): (0-1).

7. The method according to claim 1, characterized in that The step three specifically includes the following steps: Step 3.1, in a reactor equipped with linear p-cresol / o-ethylphenol phenolic resin prepolymer, add high-purity m-cresol / o-ethylphenol obtained in step 1 and a catalyst, start stirring and fully mix, and heat to 80-100° C. and add paraformaldehyde in batches for reaction, the addition time is 1-6 hours, and the temperature is kept for 1-3 hours after the addition, and sampling is analyzed. The content of m-cresol is less than 0.5% by liquid chromatography or gel chromatography analysis, which is qualified; Step 3.2, after passing the test, the temperature is raised for distillation, and the distilled material is recorded as a p-cresol / o-ethylphenol mixture aqueous solution; Step 3.3, after the unreacted cresol and o-ethylphenol are evaporated, add an acid-base amphoteric compound to the reaction mass, mix well, and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, the water level of the receiver is observed. After the water level is constant within 20 minutes, the vacuum degree is gradually increased to 0.098MPa, and the temperature is further increased for dehydration. When the material temperature in the reactor reaches 190-210°C and no liquid is distilled out, keep warm for 1-2 hours, stop dehydration, break the vacuum with nitrogen, and discharge the material to a stainless steel material tray while hot under nitrogen protection to obtain a white to light yellow meta-cresol-formaldehyde resin product as a film material for photoresist.

8. The method according to claim 7, characterized in that In step 3.1: The mass ratio of linear p-cresol / o-ethylphenol phenolic resin prepolymer to high-purity m-cresol / o-ethylphenol (0.4-0.6) is 1; the amount of catalyst added is 0.5-5% of the mass of high-purity m-cresol / o-ethylphenol; The amount of paraformaldehyde added is: the ratio of the molar amount of formaldehyde in the paraformaldehyde to the total molar amount of p-cresol and o-ethylphenol in the high-purity m-cresol / o-ethylphenol is 0.5-0.9; and the molar amount of formaldehyde in the paraformaldehyde is 0.7-0.9 times the sum of the total molar amount of p-cresol and o-ethylphenol in the high-purity m-cresol / o-ethylphenol and the total molar amount of p-cresol and o-ethylphenol in the aqueous solution of the p-cresol / o-ethylphenol mixture in step 2; In step 3.3: The amount of the acid-base amphoteric compound added is 0.1-10% of the mass of high-purity m-p-cresol / o-ethylphenol; The acid-base amphoteric compound is triethylamine acetate adduct, and the preparation method is: prepare it according to the weight ratio of triethylamine / glacial acetic acid = 5 / 6-15, add triethylamine dropwise into glacial acetic acid under stirring, control the temperature below 50°C, and after mixing, reduce the pressure and recover the mixed solvent, which is the triethylamine acetate adduct.

9. The method according to claim 7, characterized in that: In the step 3.2, the obtained p-cresol / o-ethylphenol mixture aqueous solution is used for the preparation of the next batch of linear p-cresol / o-ethylphenol novolac resin prepolymer, or the material layer is used to separate p-cresol and o-ethylphenol after layering; After the p-cresol / o-ethylphenol aqueous solution is layered, the material layer is used to separate p-cresol and o-ethylphenol, and the steps are as follows: 1) the p-cresol / o-ethylphenol mixture aqueous solution is layered to obtain a material layer, wherein the material layer is a mixture of p-cresol and o-ethylphenol; 2) Passing a mixture of p-cresol and o-ethylphenol into a fixed bed reactor preheated to 300-500°C in the presence of hydrogen for reaction, wherein a transposition catalyst is installed in the fixed bed reactor, and the p-cresol content in the material coming out of the fixed bed is controlled to be ≤25% and the o-ethylphenol content is ≤10%. The materials generated by the reaction are cooled and collected in an intermediate storage tank; 3) Transfer the material in the intermediate storage tank into the kettle of the distillation tower, and perform vacuum distillation to obtain m-p-cresol and m-p-ethylphenol.

10. The method according to claim 7, characterized in that In the step 3.3, a white to light yellow meta-cresol-formaldehyde resin product is obtained, and ethylene glycol and ethanol are added to form a solution, which is used as a film material for photoresist.