Water-soluble sizing agent as well as preparation method and application thereof
The water-soluble sulfonated product is prepared by reacting polyether ether ketone containing Cardo gene with chlorosulfonic acid. As a sizing agent for carbon fiber, the problem of insufficient interface binding ability between polyether ether ketone and carbon fiber is solved, and the composite material is significantly improved Mechanical properties.
Patent Information
- Application Number
- CN202411218710.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The application of polyether ether ketone in the field of sizing agents is limited by its inertness and high viscosity, which leads to insufficient interfacial binding ability with carbon fibers, affecting the performance of composite materials.
A water-soluble sulfonated product is prepared by reacting polyether ether ketone containing Cardo gene with chlorosulfonic acid. As a sizing agent for carbon fibers, its solubility in water and compatibility with carbon fibers are improved by sulfonation treatment.
The bonding of carbon fiber and polyether ether ketone resin is improved, the mechanical properties of composite materials are enhanced, and better application prospects are achieved.
Smart Images

Figure CN118930778A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of carbon fiber technology, and in particular to a water-soluble sizing agent and a preparation method and application thereof. Background Art
[0002] Carbon fiber is a one-dimensional carbon material with the characteristics of high specific strength, high specific modulus, high temperature resistance, and low density. It is a typical reinforcement. Polyetheretherketone is an aromatic semi-crystalline high-performance thermoplastic polymer with the characteristics of radiation resistance, hydrolysis resistance, corrosion resistance, high temperature resistance, wear resistance, and fatigue resistance. It is one of the high-performance engineering plastics that is widely used in the field of materials. Since it is difficult to meet the requirements of the field of high-tech materials by using polyetheretherketone alone, in order to further improve the comprehensive performance of polyetheretherketone, carbon fiber can be used to enhance its performance. Polyetheretherketone-based carbon fiber reinforced composites are ideal materials for aerospace, aviation, automobiles and other fields. However, polyetheretherketone itself is inert, the surface activity of carbon fiber is also low, and the viscosity of polyetheretherketone is high. These factors affect the interface between the two and affect the performance of the composite material. Therefore, improving the interface bonding ability between the two is the focus of the design and preparation of composite materials.
[0003] Sizing treatment can improve the surface properties of carbon fiber and the interfacial compatibility between carbon fiber and matrix resin, thereby improving the interfacial properties of carbon fiber resin-based composite materials. For different composite material systems, it is necessary to select a sizing agent that matches the matrix resin to sizing the carbon fiber in order to give full play to the reinforcing effect of the carbon fiber. However, the advantage of ordinary polyetheretherketone that it is insoluble in any single-component solvent except concentrated sulfuric acid at room temperature has become the biggest obstacle to its application in the field of sizing agents. Using concentrated sulfuric acid to dissolve polyetheretherketone and then sizing the carbon fiber has high equipment requirements and low safety. Summary of the invention
[0004] The present application provides a water-soluble sizing agent and a preparation method and application thereof, which can be dissolved in water to form a stable aqueous solution, thereby being used as a carbon fiber sizing agent to improve the mechanical properties of a composite material formed with the carbon fiber.
[0005] The embodiment of the present application is implemented as follows:
[0006] In a first aspect, the present application provides a method for preparing a water-soluble sizing agent, which comprises: reacting polyetheretherketone containing a Cardo gene and chlorosulfonic acid at a temperature of 30° C. to 40° C. for 60 min to 80 min.
[0007] The chemical formula of polyetheretherketone containing Cardo gene is as follows:
[0008]
[0009] In the above technical scheme, the present application uses polyetheretherketone containing Cardo gene as raw material, polyetheretherketone containing Cardo gene can be well dissolved in organic solvent, polyetheretherketone containing Cardo gene is sulfonated by chlorosulfonic acid, and the obtained product can be well dissolved in water, and it can be used as a sizing agent for carbon fiber without emulsification and other operations. At the same time, the sulfonated polyetheretherketone containing Cardo gene and polyetheretherketone matrix resin have good compatibility, can improve the binding property of polyetheretherketone matrix resin and carbon fiber, enhance the interface effect, and then can improve the mechanical properties of the composite material formed by polyetheretherketone matrix resin and carbon fiber, and has good application prospects.
[0010] In some embodiments, the mass ratio of polyetheretherketone containing the Cardo gene to chlorosulfonic acid is 5-10:90-95.
[0011] In the above example, by making the mass ratio of the cardo gene-containing polyetheretherketone and chlorosulfonic acid within the above range, it is possible to obtain a sulfonated cardo gene-containing polyetheretherketone having good water solubility.
[0012] In some embodiments, stirring is maintained during the reaction of the polyetheretherketone containing the Cardo gene and chlorosulfonic acid, and the stirring rate is 500 r / min to 1000 r / min.
[0013] In some embodiments, after the reaction is completed, the obtained mixture is cooled to below 0° C., a solid is precipitated, the solid is collected, and the solid is washed with an alkaline solution.
[0014] In the above example, the sulfonated polyetheretherketone containing the Cardo gene can be precipitated below 0°C, and the alkaline solution can neutralize the excess chlorosulfonic acid in the solid matter to improve the purity of the product.
[0015] In some embodiments, the alkaline solution includes sodium hydroxide and / or potassium hydroxide.
[0016] In some embodiments, during the process of washing the solids with an alkaline solution, a pH meter is used to track the pH value of the washing solution, and washing is completed when the pH value remains unchanged.
[0017] In the above example, using a pH meter to track the pH value of the washing liquid can accurately determine whether the excess chlorosulfonic acid in the solid matter has been neutralized, which is beneficial to improving the purity of the product and reducing production costs.
[0018] In some embodiments, after washing is completed, the washed solid is filtered using a dialysis membrane and then freeze-dried to obtain the sulfonated Cardo gene-containing polyetheretherketone.
[0019] In some embodiments, the dialysis membrane has a cut-off of 3 kDa.
[0020] In the above example, the dialysis membrane retains the desired product and removes unreacted starting materials.
[0021] In a second aspect, the present application example provides a water-soluble sizing agent, which is prepared according to the preparation method of the water-soluble sizing agent in the above embodiment of the claim.
[0022] In the above technical solution, the water-soluble sizing agent of the present application can be well dissolved in water, and can be used as a sizing agent for carbon fiber without further emulsification and other operations. At the same time, the water-soluble sizing agent can be well combined with carbon fiber, enhance the interface effect, and further improve the mechanical properties of the composite material formed with carbon fiber, and has good application prospects.
[0023] In a third aspect, the present application provides an example of using the water-soluble sizing agent in the above embodiment in preparing a carbon fiber composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 This is the infrared spectrum of the sulfonated polyetheretherketone containing the Cardo gene obtained in Example 1 of the present application. DETAILED DESCRIPTION
[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] The following is a specific description of a water-soluble sizing agent and its preparation method and application according to an embodiment of the present application:
[0028] The present invention provides a method for preparing a water-soluble sizing agent, which comprises the following steps:
[0029] S1. Synthesis
[0030] The polyetheretherketone containing the Cardo gene and chlorosulfonic acid are reacted at a temperature of 30° C. to 40° C. for 60 min to 80 min.
[0031] The chemical formula of polyetheretherketone containing Cardo gene is as follows:
[0032]
[0033] Among them, n is 5 to 100.
[0034] As an example, the reaction temperature of the cardo gene-containing polyetheretherketone and chlorosulfonic acid can be 30° C., 31° C., 32° C., 33° C., 34° C., 35° C., 36° C., 37° C., 38° C., 39° C., or 40° C. The reaction time of the cardo gene-containing polyetheretherketone and chlorosulfonic acid can be 60 min, 65 min, 70 min, 75 min, or 80 min.
[0035] In some embodiments, the mass ratio of polyetheretherketone containing the Cardo gene to chlorosulfonic acid is 5-10:90-95.
[0036] As an example, the mass ratio of polyetheretherketone containing Cardo gene and chlorosulfonic acid can be 10:90, 9:91, 8:92, 7:93, 6:94 or 5:95.
[0037] By making the mass ratio of the cardo gene-containing polyetheretherketone and chlorosulfonic acid within the above range, it is possible to obtain a sulfonated cardo gene-containing polyetheretherketone having good water solubility.
[0038] In some embodiments, stirring is maintained during the reaction of the polyetheretherketone containing the Cardo gene and chlorosulfonic acid, and the stirring rate is 500 r / min to 1000 r / min.
[0039] As an example, the stirring rate during the reaction of the Cardo gene-containing polyetheretherketone and chlorosulfonic acid may be 500 r / min, 600 r / min, 700 r / min, 800 r / min, 900 r / min, or 1000 r / min.
[0040] S2. Precipitation
[0041] After the reaction is completed, the obtained mixture is cooled to below 0° C. to precipitate a solid, which is collected and washed with an alkaline solution.
[0042] Sulfonated polyetheretherketone containing Cardo gene can be precipitated below 0°C, and alkaline solution can neutralize excess chlorosulfonic acid in the solid matter to improve the purity of the product.
[0043] In some embodiments, the alkaline solution includes sodium hydroxide and / or potassium hydroxide.
[0044] As examples, the alkaline solution may be sodium hydroxide alone, or potassium hydroxide alone, or a mixture of sodium hydroxide and potassium hydroxide.
[0045] It should be noted that the alkaline solution of the present application is not limited to the above substances, as long as it is a strong base.
[0046] In some embodiments, during the process of washing the solids with an alkaline solution, a pH meter is used to track the pH value of the washing solution, and washing is completed when the pH value remains unchanged.
[0047] Using a pH meter to track the pH value of the washing liquid can accurately determine whether the excess chlorosulfonic acid in the solid matter has been neutralized, which is beneficial to improving the purity of the product and reducing production costs.
[0048] S3. Filtering
[0049] After washing is completed, the washed solid is filtered using a dialysis membrane and then freeze-dried to obtain the sulfonated Cardo gene-containing polyetheretherketone.
[0050] In some embodiments, the dialysis membrane has a cut-off of 3 kDa.
[0051] S4. Preparation of water-soluble sizing agent
[0052] The prepared sulfonated polyetheretherketone containing Cardo gene is dissolved in water to prepare a water-soluble sizing agent.
[0053] It should be noted that the mass percentage of the sulfonated polyetheretherketone containing the Cardo gene in the water-soluble sizing agent can be adjusted according to actual needs.
[0054] This application uses Cardo gene-containing polyetheretherketone as a raw material. Cardo gene-containing polyetheretherketone can be well dissolved in an organic solvent. Chlorosulfonic acid is used to sulfonate the Cardo gene-containing polyetheretherketone. The obtained product can be well dissolved in water and can be used as a sizing agent for carbon fiber without emulsification and other operations. At the same time, the sulfonated Cardo gene-containing polyetheretherketone and polyetheretherketone matrix resin have good compatibility, can improve the binding of polyetheretherketone matrix resin and carbon fiber, enhance the interface effect, and then can improve the mechanical properties of the composite material formed by polyetheretherketone matrix resin and carbon fiber, and has good application prospects.
[0055] The present application also provides a water-soluble sizing agent, which is prepared according to the preparation method of the water-soluble sizing agent in the above embodiment of the claim.
[0056] The water-soluble sizing agent of the present application can be well dissolved in water, and can be used as a sizing agent for carbon fiber without the need for emulsification or other operations. At the same time, the water-soluble sizing agent can be well combined with carbon fiber, enhance the interface effect, and further improve the mechanical properties of the composite material formed with the carbon fiber, and has good application prospects.
[0057] The present application also provides a use of the water-soluble sizing agent in the above embodiment in preparing a carbon fiber composite material.
[0058] The following is a further detailed description of a water-soluble sizing agent of the present application and its preparation method and application in conjunction with embodiments.
[0059] Example 1
[0060] The present invention provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0061] S1. Synthesis
[0062] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 35°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 70 minutes.
[0063] S2. Precipitation
[0064] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0065] S3. Filtering
[0066] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing the Cardo gene (sulfonated PEEK-WC). The infrared spectrum of the obtained sulfonated polyetheretherketone containing the Cardo gene is as follows: Figure 1 shown.
[0067] S4. Preparation of aqueous sizing agent
[0068] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0069] S5. Application
[0070] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0071] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0072] Example 2
[0073] The present invention provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0074] S1. Synthesis
[0075] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 40°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 60 minutes.
[0076] S2. Precipitation
[0077] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0078] S3. Filtering
[0079] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0080] S4. Preparation of aqueous sizing agent
[0081] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0082] S5. Application
[0083] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0084] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0085] Example 3
[0086] The present invention provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0087] S1. Synthesis
[0088] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 30°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 80 minutes.
[0089] S2. Precipitation
[0090] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0091] S3. Filtering
[0092] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0093] S4. Preparation of aqueous sizing agent
[0094] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0095] S5. Application
[0096] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0097] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0098] Example 4
[0099] The present invention provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0100] S1. Synthesis
[0101] 97.5 parts by weight of chlorosulfonic acid and 2.5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 35°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 70 minutes.
[0102] S2. Precipitation
[0103] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0104] S3. Filtering
[0105] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0106] S4. Preparation of aqueous sizing agent
[0107] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0108] S5. Application
[0109] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0110] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0111] Example 5
[0112] The present invention provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0113] S1. Synthesis
[0114] 90 parts by weight of chlorosulfonic acid and 10 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 35°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 70 minutes.
[0115] S2. Precipitation
[0116] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0117] S3. Filtering
[0118] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0119] S4. Preparation of aqueous sizing agent
[0120] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0121] S5. Application
[0122] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0123] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0124] Comparative Example 1
[0125] The comparative example of the present application provides an application of a common epoxy-based sizing agent, which comprises the following steps:
[0126] The unsized T700 carbon fiber is immersed in a common epoxy sizing agent for 2 minutes through a surface sizing treatment device, and then dried at high temperature in vacuum to obtain the sized T700 carbon fiber.
[0127] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0128] Comparative Example 2
[0129] The comparative example of the present application provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0130] S1. Synthesis
[0131] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 20°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 70 minutes.
[0132] S2. Precipitation
[0133] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0134] S3. Filtering
[0135] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0136] S4. Preparation of aqueous sizing agent
[0137] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0138] S5. Application
[0139] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0140] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0141] Comparative Example 3
[0142] The comparative example of the present application provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0143] S1. Synthesis
[0144] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 50°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 70 minutes.
[0145] S2. Precipitation
[0146] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0147] S3. Filtering
[0148] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0149] S4. Preparation of aqueous sizing agent
[0150] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0151] S5. Application
[0152] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0153] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0154] Comparative Example 4
[0155] The comparative example of the present application provides a water-soluble sizing agent and a preparation method and application thereof, which comprises the following steps:
[0156] S1. Synthesis
[0157] 95 parts by weight of chlorosulfonic acid and 5 parts by weight of polyetheretherketone (PEEK-WC) powder containing Cardo gene were added to the reaction container respectively, and the reaction container was placed in a constant temperature water bath, the temperature was set to 35°C, the stirring rate was 800r / min, and the reaction was maintained under stirring for 40 minutes.
[0158] S2. Precipitation
[0159] After the reaction is completed, the obtained mixture is cooled to below 0°C, the precipitated solid is collected by filtration to obtain a solid, and the solid is washed with a sodium hydroxide solution to neutralize excess chlorosulfonic acid in the solid until the pH value of the solution remains unchanged.
[0160] S3. Filtering
[0161] After washing, the washed solid was filtered to remove inorganic salts using a dialysis membrane with a cutoff of 3 kDa, and then freeze-dried to obtain sulfonated polyetheretherketone containing Cardo gene (sulfonated PEEK-WC).
[0162] S4. Preparation of aqueous sizing agent
[0163] The prepared sulfonated polyetheretherketone containing Cardo gene was dissolved in water to prepare a water-soluble sizing agent with a mass percentage of 1.0%wt.
[0164] S5. Application
[0165] The unsized T700 carbon fiber is immersed in the prepared water-soluble sizing agent with a mass percentage of 1.0%wt for 2 minutes through a surface sizing treatment device, and then dried in vacuum at high temperature to obtain the sized T700 carbon fiber.
[0166] The sized T700 carbon fiber and polyetheretherketone resin (PEEK) are prepared into prepreg by a powder impregnation method, and the prepared prepreg is cut, laid and molded to obtain a carbon fiber reinforced PEEK-based composite material.
[0167] Test Example 1
[0168] The composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were tested for interlaminar shear strength according to ASTM D 2344, for compression strength according to ASTM D6641, and for flexural strength according to ASTM D7264. The results are shown in Table 1.
[0169] Table 1 Properties of the composite materials obtained in Examples 1 to 5 and Comparative Examples 1 to 4
[0170] project Interlaminar shear strength (MPa) Compression strength(MPa) Bending strength(MPa) Example 1 90 1365 1958 Example 2 92 1313 1874 Example 3 91 1401 1910 Example 4 88 1448 1811 Example 5 93 1350 1898 Comparative Example 1 65 1109 1577 Comparative Example 2 68 1084 1577 Comparative Example 3 57 1132 1505 Comparative Example 4 52 1015 1422
[0171] It can be seen from Examples 1 to 5 that the composite material prepared by using the water-soluble sizing agent of the present application has an interlaminar shear strength of ≥88 MPa, a compression strength of ≥1313 MPa, and a flexural strength of ≥1811 MPa.
[0172] From the comparison between Example 1 and Comparative Example 1, it can be seen that after Example 1 uses sulfonated PEEK-WC as a sizing agent, compared with Comparative Example 1 using a common epoxy-based sizing agent, the interlaminar shear strength, compressive strength and flexural strength of the composite material prepared are greatly improved.
[0173] From the comparison between Example 1 and Comparative Example 2, it can be seen that the reaction temperature of polyetheretherketone containing Cardo gene and chlorosulfonic acid in Comparative Example 2 is only 20°C. Compared with Example 1, the interlaminar shear strength, compressive strength and flexural strength of the prepared composite material are all reduced.
[0174] From the comparison between Example 1 and Comparative Example 3, it can be seen that the reaction temperature of polyetheretherketone containing Cardo gene and chlorosulfonic acid in Comparative Example 3 is as high as 50°C. Compared with Example 1, the interlaminar shear strength, compressive strength and flexural strength of the prepared composite material are all reduced.
[0175] From the comparison between Example 1 and Comparative Example 4, it can be seen that the reaction time of polyetheretherketone containing Cardo gene and chlorosulfonic acid in Comparative Example 4 is only 40 minutes. Compared with Example 1, the interlaminar shear strength, compressive strength and flexural strength of the prepared composite material are all reduced.
[0176] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a water-soluble sizing agent, characterized in that: The preparation method of the water-soluble sizing agent comprises: reacting polyetheretherketone containing Cardo gene and chlorosulfonic acid at a temperature of 30° C. to 40° C. for 60 min to 80 min; The chemical formula of the polyetheretherketone containing the Cardo gene is as follows:
2. The method for preparing a water-soluble sizing agent according to claim 1, characterized in that: The mass ratio of the polyetheretherketone containing the Cardo gene to the chlorosulfonic acid is 5-10:90-95.
3. The method for preparing a water-soluble sizing agent according to claim 1, characterized in that: During the reaction of the polyetheretherketone containing the Cardo gene and the chlorosulfonic acid, stirring is maintained at a rate of 500 r / min to 1000 r / min.
4. The method for preparing a water-soluble sizing agent according to claim 1, characterized in that: After the reaction is completed, the obtained mixture is cooled to below 0° C. to precipitate solids, which are collected and washed with an alkaline solution.
5. The method for preparing a water-soluble sizing agent according to claim 4, characterized in that: The alkaline solution includes sodium hydroxide and / or potassium hydroxide.
6. The method for preparing a water-soluble sizing agent according to claim 4, characterized in that: In the process of washing the solid matter with the alkaline solution, a pH meter is used to track the pH value of the washing solution, and the washing is completed when the pH value remains unchanged.
7. The method for preparing a water-soluble sizing agent according to claim 4, characterized in that: After the washing is completed, the washed solid is filtered using a dialysis membrane and then freeze-dried to obtain the sulfonated polyetheretherketone containing the Cardo gene.
8. The method for preparing a water-soluble sizing agent according to claim 7, characterized in that: The cut-off of the dialysis membrane was 3 kDa.
9. A water-soluble sizing agent, characterized in that: The water-soluble sizing agent is prepared according to the preparation method of the water-soluble sizing agent according to any one of claims 1 to 8.
10. Use of the water-soluble sizing agent according to claim 9 in preparing carbon fiber composite materials.
Citation Information
Cited By
Environment-friendly water-based thermoplastic carbon fiber sizing agent and preparation method thereof
CN121228530A