Flame-retardant hard foam polyether polyol as well as preparation method and application thereof

The flame-retardant hard foam polyether polyol is prepared by polymerizing the polyurethane hard foaming materials with silane compounds containing primary amino groups and diphenylphosphorus chloride with olefin oxide, which solves the difficulty of improving insulation and flame retardant at the same time in the existing materials. The problem of strength and achieves the high flame retardancy and strength of polyurethane hard bubbles, and is suitable for applications such as refrigerated trucks and refrigerated containers.

CN118930836AActive Publication Date: 2024-11-12WANHUA CHEMYANTAI RONGWEI POLYURETHANE CO LTD +2

Patent Information

Application Number
CN202411244157.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing polyurethane hard foam materials are difficult to improve insulation performance, flame retardant performance and strength support performance at the same time, and cannot meet the high requirements of refrigerated trucks and refrigerated containers for safety performance and comprehensive material performance.

Method used

Flame-retardant hard foamed polyether polyol is prepared by polymerizing with oxyolefins using silane compounds containing primary amine groups and diphenylphosphorus chloride as starting agents, reducing the surface tension of the foaming system, improving compatibility and The delicate structure of the cell enhances the flame retardancy and strength of the foam.

Benefits of technology

It realizes smooth foaming of polyurethane hard foam, improves the compressive strength and bending strength of the foam, while maintaining a low thermal conductivity and high oxygen index, meeting the high flame retardancy and strength requirements in fields such as refrigeration trucks and refrigerated containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005030152150000091
    Figure BDA0005030152150000091
  • Figure BDA0005030152150000101
    Figure BDA0005030152150000101
  • Figure BDA0005030152150000111
    Figure BDA0005030152150000111
Patent Text Reader

Abstract

The invention discloses flame-retardant hard foam polyether polyol as well as a preparation method and application thereof. The preparation method of the polyether polyol comprises the following steps: taking a silane compound containing a primary amino group and diphenyl phosphorus halide as raw materials, and reacting under an alkaline condition to obtain an intermediate; and carrying out polymerization reaction on the intermediate serving as an initiator and oxyalkylene under the action of a polymerization catalyst to prepare the polyether polyol. The polyether polyol obtained by the invention is prepared by taking reactants of a silane compound containing primary amino and diphenyl phosphorus chloride as initiators and carrying out polymerization reaction on the initiators and oxyalkylene, and the particularity of a molecular structure is beneficial to reducing the surface tension of a foaming system and improving the compatibility, so that the foaming process is stable and controllable, the foam structure is finer and smoother, and the foaming effect is better. Meanwhile, the foam strength is high, and the flame retardance is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyether polyol, in particular to a flame retardant rigid foam polyether polyol and a preparation method and application thereof. Background Art

[0002] Polyurethane rigid foam materials are widely used in insulation fields such as refrigerators, freezers, refrigerated trucks, and refrigerated containers due to their extremely low thermal conductivity, high compression strength, and simple production process. Among them, refrigerated trucks and refrigerated containers are important transportation carriers for cold chain logistics. The market has increasingly higher requirements for the safety performance, stability of use, and flame retardant properties of refrigerated trucks. This requires polyurethane rigid foam to have not only good thermal insulation and flame retardant properties, but also strength support. It is difficult to improve the comprehensive performance of the above multiple aspects at the same time with current technology. Summary of the invention

[0003] In order to solve the above technical problems, the present invention first proposes a flame retardant rigid foam polyether polyol and a preparation method thereof. The polyether polyol is prepared by polymerization reaction of a silane compound containing a primary amino group and diphenylphosphonium chloride as an initiator with an oxidized olefin, and the particularity of the molecular structure is conducive to reducing the surface tension of the foaming system, improving the compatibility, making the foaming process stable and controllable, and the pore structure is more delicate, while the foam strength is high and the flame retardancy is good.

[0004] Secondly, the present invention also provides an application of a flame retardant rigid foam polyether polyol in preparing a polyurethane rigid foam. The obtained polyurethane rigid foam has many of the above advantages.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] As a first aspect of the present invention, a method for preparing a flame retardant rigid foam polyether polyol is provided, comprising the following steps:

[0007] A silane compound containing a primary amino group and a diphenylphosphonium halide are used as raw materials to react under alkaline conditions to obtain an intermediate; then the intermediate is used as an initiator to undergo a polymerization reaction with an oxidized olefin under the action of a polymerization catalyst to obtain a polyether polyol.

[0008] In some preferred preparation methods,

[0009] The molar ratio of the silane compound to the diphenylphosphorus halide is 1-3:1;

[0010] Preferably, the silane compound is selected from one or more of 3-aminopropyltriethoxysilane, (3-aminopropyl)dimethylmethoxysilane, (3-aminoethyl)dimethylmethoxysilane;

[0011] Preferably, the phenyl phosphorus halide is selected from one or more of diphenyl phosphorus chloride, phenyl phosphorus dichloride, (2-chlorophenyl) diphenylphosphine;

[0012] Preferably, the alkaline conditions for the reaction of the silane compound and the diphenylphosphonium halide are provided by an organic base and / or an inorganic base; the organic base is selected from one or more of triethylamine, dimethylethylamine, and diisopropylethylamine; the inorganic base is selected from one or more of sodium methoxide, potassium ethoxide, and potassium tert-butoxide;

[0013] The amount of the organic base and / or inorganic base used is 0.5-2 times the molar amount of the silane compound.

[0014] In some preferred preparation methods, the olefin oxide is one or more of ethylene oxide, propylene oxide, butylene oxide, and tetrahydrofuran;

[0015] Preferably, the amount of the olefin oxide is 2-8 times the molar amount of the corresponding silane compound;

[0016] Preferably, the polymerization catalyst is an alkaline catalyst and / or a bimetallic complex catalyst, more preferably one or more of potassium hydroxide, sodium hydroxide, potassium alcoholate, sodium alcoholate, MMC, and DMC;

[0017] Preferably, the amount of the polymerization catalyst used is 1-3% of the mass of the corresponding silane compound.

[0018] In some preferred preparation methods, the reaction temperature of the silane compound and diphenylphosphorus halide is 35-45° C., and the reaction time is 1-3 hours;

[0019] Preferably, the polymerization reaction is divided into an esterification addition reaction stage and a vacuum aging stage, wherein the esterification addition reaction is a reaction of a silane compound and a polymerization catalyst in a reactor completely replaced with nitrogen, with stirring and heating to 120-150°C, and adding oxidized olefins to react for 1-4 hours; after the esterification addition reaction is completed, the temperature is raised to 180-200°C, and vacuum aging is carried out while maintaining the pressure at no more than 0.8 MPa to evaporate the by-product water and unreacted oxidized olefins.

[0020] The above polymerization reaction process is relatively conventional and easy to adjust for those skilled in the art without considering the selection of initiator. For details, reference may be made to various schemes disclosed in known technologies, and no specific limitation is made here.

[0021] It is worth noting that the reaction completion degree of the silane compound and the diphenylphosphonium halide is relatively high. Based on the consideration of saving the reaction process, the unreacted raw materials can be directly put into the polymerization reaction for the next step of reaction without separation, and the light components can be removed once in the vacuum polycondensation stage.

[0022] In addition, after the polymerization reaction is completed and the aging is finished, the polyether polyol is obtained by conventional post-treatment processes such as neutralization, adsorption dehydration, and filtration. Available neutralizers include phosphoric acid, lactic acid, acetic acid, etc.; available adsorbents include magnesium silicate, magnesium polysilicate, aluminum polysilicate, diatomaceous earth, etc.; available filtering equipment includes vacuum filters, preferably filtering at a vacuum of -0.09Mpa, and the filtering time is, for example, 0.5-1h. After filtering, the filtrate is collected to obtain the polyether polyol.

[0023] As a second aspect of the present invention, there is also provided a flame retardant rigid foam polyether polyol prepared by the method described above, which has a functionality of 1, a hydroxyl value of 70-120 mgKOH / g, and a viscosity of 400-800 mPa*s at 25°C.

[0024] As a third aspect of the present invention, a flame retardant polyurethane rigid foam is also provided, comprising a polyisocyanate component and a combined polyether component, wherein the combined polyether component comprises A) a polyol, B) a blowing agent and optionally C) an auxiliary agent;

[0025] Wherein, A) the polyol comprises the flame retardant rigid foam polyether polyol prepared by the method described above; preferably, the mass content of the flame retardant rigid foam polyether polyol prepared by the method described above in A) the polyol is 5-40wt%.

[0026] In some preferred embodiments of the invention, the mass ratio of the polyisocyanate component to the combined polyether component is (1-1.5):1;

[0027] Preferably, the polyisocyanate component is polymeric MDI or liquefied modified MDI, preferably one or more of Wanhua PM200, PM400, and PM700;

[0028] Preferably, B) the amount of the foaming agent is 5-15% by mass of the combined polyether component;

[0029] Preferably, the amount of C) the auxiliary agent is 10-20% by weight of the combined polyether component.

[0030] In some preferred embodiments of the invention, A) the polyol optionally further comprises at least one of a polyether polyol with sucrose as an initiator, a polyether polyol with sorbitol as an initiator, a polyether polyol with propylene glycol as an initiator, and a polyester polyol with phthalic anhydride as an initiator;

[0031] Preferably, the polyether polyol using sucrose as the initiator is a polyether polyol prepared by polymerization of propylene oxide and / or ethylene oxide using sucrose as the initiator, with a molecular weight of 300-800, a functionality of 4.5-6, and a hydroxyl value of 300-420 mgKOH / g; preferably, the mass fraction of the polyether polyol using sucrose as the initiator in A) is ≤40wt% (e.g., 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, etc.), preferably 5-40wt%;

[0032] Preferably, the polyether polyol using sorbitol as an initiator is a polyether polyol prepared by polymerization of propylene oxide and / or ethylene oxide using sorbitol as an initiator, with a molecular weight of 600-700, a functionality of 4.5-6, and a hydroxyl value of 400-500 mgKOH / g; preferably, the mass fraction of the polyether polyol using sorbitol as an initiator in A) is ≤30wt% (e.g., 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, etc.), preferably 5-30wt%;

[0033] Preferably, the polyether polyol with propylene glycol as the initiator is a polyether polyol prepared by polymerization of propylene glycol as the initiator with propylene oxide and / or ethylene oxide, with a molecular weight of 400-1000, a functionality of 1.5-2, and a hydroxyl value of 400-800 mgKOH / g; preferably, the mass fraction of the polyether polyol with propylene glycol as the initiator in A) is ≤30wt% (e.g., 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, etc.), preferably 5-30wt%.

[0034] Preferably, the polyester polyol using phthalic anhydride as the initiator has a molecular weight of 300-500, a functionality of 2, and a hydroxyl value of 220-350 mgKOH / g; the polyester polyol using phthalic anhydride as the initiator is preferably one or more of Stepan PS-3152, PS-2452, and PS-2352; preferably, the mass fraction of the polyester polyol using phthalic anhydride as the initiator in A) the polyol is ≤20wt% (e.g., 5wt%, 10wt%, 15wt%, 20wt%, etc.), preferably 5-20wt%.

[0035] In some preferred embodiments of the present invention, the blowing agent is one or more of cyclopentane, isopentane, and n-pentane, or a mixture of at least one of cyclopentane, isopentane, and n-pentane and water.

[0036] In some preferred embodiments of the invention, the auxiliary agent is one or more of a flame retardant, a surfactant, and a catalyst;

[0037] Preferably, the flame retardant is tris(chloroisopropyl)phosphate and / or triethyl phosphate;

[0038] Preferably, the surfactant is a siloxane, preferably one or more of B8546, B84813, AK88310, AK88719;

[0039] Preferably, the catalyst is an amine and / or a metal salt and / or water, more preferably one or more of pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, triethylenediamine, TMR-2, N,N-dimethylbenzylamine, potassium formate, potassium acetate, potassium isooctanoate, and water.

[0040] Finally, the present invention also provides a method for preparing a flame retardant polyurethane rigid foam, comprising the following steps:

[0041] (1) uniformly mixing a polyol, a blowing agent and optionally an auxiliary agent to obtain a combined polyether component;

[0042] (2) mixing the combined polyether component and the polyisocyanate component to form a foam;

[0043] In some preferred embodiments, the mixed foaming temperature of the combined polyether component and the polyisocyanate component is 15-25°C.

[0044] The polyurethane rigid foam provided by the present invention has stable gel time and foam core density, a stable and controllable foaming process, and good industrial applicability. More importantly, while maintaining a low thermal conductivity and a high oxygen index, the polyurethane foam still has improved compression strength and bending strength, so the foam has the advantages of fine pores, high strength, and good flame retardancy, and can be widely used in the field of thermal insulation material preparation, such as refrigerated container insulation layer, refrigerated truck insulation layer, etc. DETAILED DESCRIPTION

[0045] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0046] Unless otherwise specified, the raw material information in the following embodiments are all from common commercially available products.

[0047] Polyether polyol A1: 3-aminopropyl triethoxysilane and diphenylphosphonium chloride are added dropwise in a molar ratio of 1:1 for reaction, and triethylamine is used in an amount of 1 times the molar amount of 3-aminopropyl triethoxysilane to provide an alkaline environment for the reaction; react at room temperature for two hours to obtain an intermediate. The intermediate and potassium hydroxide are mixed in a reactor, wherein the amount of potassium hydroxide is 1% of the mass of 3-aminopropyl triethoxysilane, and nitrogen is replaced and vacuumed, and then stirred and heated to 120°C, and then part of propylene oxide (accounting for 10% of the total mass of propylene oxide) is added, and the total molar amount of propylene oxide is 5 times the molar amount of 3-aminopropyl triethoxysilane, and matured for 2 hours; after the aging is completed, the remaining amount of propylene oxide is added and the temperature is raised to 150°C, the pressure is maintained at 0.8MPa, and the polymerization reaction is carried out for 2 hours, and then vacuumed and matured to remove light component impurities. After aging, phosphoric acid was added for neutralization, and magnesium silicate was added for adsorption and dehydration. After stirring, the mixture was filtered to obtain polyether polyol A1; the functionality was 1, the hydroxyl value was 100 mgKOH / g, and the viscosity was 600 mpa*s.

[0048] Polyether polyol A2: 3-aminopropyl triethoxysilane and phenylphosphonium dichloride are added dropwise in a molar ratio of 1:1 for reaction, and triethylamine is used in an amount of 1 times the molar amount of 3-aminopropyl triethoxysilane to provide an alkaline environment for the reaction; react at room temperature for two hours to obtain an intermediate. The intermediate and DMC are mixed in a reactor, wherein the amount of DMC is 2% of the mass of 3-aminopropyl triethoxysilane, and the reactor is evacuated by nitrogen replacement, and then stirred and heated to 130°C, and then part of propylene oxide (accounting for 10% of the total mass of propylene oxide) is added, and the total molar amount of propylene oxide is 8 times the molar amount of 3-aminopropyl triethoxysilane, and matured for 2 hours; after the aging is completed, the remaining amount of propylene oxide is added and the temperature is raised to 150°C, the pressure is maintained at 0.8MPa, and the polymerization reaction is carried out for 2 hours, and then vacuumed and matured to remove light component impurities. After aging, phosphoric acid was added for neutralization, and magnesium silicate was added for adsorption and dehydration. After stirring, the mixture was filtered to obtain polyether polyol A2; the functionality was 1, the hydroxyl value was 75 mgKOH / g, and the viscosity was 750 mpa*s.

[0049] Polyether polyol A3: (3-aminopropyl) dimethylmethoxysilane and diphenylphosphonium chloride are added dropwise at a molar ratio of 2.5:1 for reaction, and triethylamine is used in an amount of 1 times the molar amount of (3-aminopropyl) dimethylmethoxysilane to provide an alkaline environment for the reaction; react at room temperature for two hours to obtain an intermediate. The intermediate and sodium hydroxide are mixed in a reactor, wherein the amount of sodium hydroxide is 3% of the mass of (3-aminopropyl) dimethylmethoxysilane, and nitrogen is replaced and vacuumed, and then stirred and heated to 150°C, and then part of propylene oxide (accounting for 10% of the total mass of propylene oxide) is added, and the total molar amount of propylene oxide is 3 times the molar amount of (3-aminopropyl) dimethylmethoxysilane, and matured for 2 hours; after the aging is completed, the remaining amount of propylene oxide is added and the temperature is raised to 180°C, the pressure is maintained at 0.8MPa, and the polymerization reaction is carried out for 2 hours, and then vacuumed and matured to remove light component impurities. After aging, phosphoric acid was added for neutralization, and magnesium silicate was added for adsorption and dehydration. After stirring, the mixture was filtered to obtain polyether polyol A3; the functionality was 1, the hydroxyl value was 118 mgKOH / g, and the viscosity was 420 mpa*s.

[0050] Polyether polyol B1: R2839, with sucrose as the initiator, hydroxyl value 380mgKOH / g, functionality 5.5, viscosity 11000mpa*s, Wanhua Chemical (Yantai) Rongwei

[0051] Polyether polyol B2: R4110, with sucrose as initiator, hydroxyl value 440mgKOH / g, functionality 4, viscosity 3000mpa*s, Wanhua Chemical (Yantai) Rongwei

[0052] Polyether polyol C1: R2380, with sorbitol as initiator, hydroxyl value 480mgKOH / g, functionality 5.4, viscosity 25000mpa*s, Wanhua Chemical (Yantai) Rongwei

[0053] Polyether polyol C2: R6245, with sorbitol as initiator, hydroxyl value 450mgKOH / g, functionality 5.4, viscosity 23000mpa*s, Wanhua Chemical (Yantai) Rongwei

[0054] Polyether polyol D1: A210, with propylene glycol as initiator, hydroxyl value 110mgKOH / g, functionality 2, viscosity 250mpa*s, Wanhua Chemical (Yantai) Rongwei

[0055] Polyether polyol D2: C2004, with propylene glycol as initiator, hydroxyl value 280mgKOH / g, functionality 2, viscosity 80mpa*s, Wanhua Chemical (Yantai) Rongwei

[0056] Polyester polyol E1: PS-2352, with phthalic anhydride as initiator, functionality 2, hydroxyl value 235 mgKOH / g, viscosity 3500 mp*s, Stepan

[0057] Polyester polyol E2: PS-3152, with phthalic anhydride as initiator, functionality 2, hydroxyl value 315mgKOH / g, viscosity 4200mp*s, Stepan

[0058] TCPP flame retardant: Yak Technology

[0059] B8546 Silicone Oil: Evonik Specialty Chemicals (Shanghai) Co., Ltd.

[0060] Composite catalyst A: a mixture of pentamethyldiethylenetriamine, dimethylcyclohexylamine, and TMR-2 in a mass ratio of 1:5:1, Evonik Specialty Chemicals (Shanghai) Co., Ltd.

[0061] Composite catalyst B: a mixture of bis(dimethylaminoethyl)ether, dimethylcyclohexylamine, and potassium acetate in a mass ratio of 1:10:2, Evonik Specialty Chemicals (Shanghai) Co., Ltd.

[0062] Cyclopentane: Meilong Chemical

[0063] n-Pentane: Meilong Chemical

[0064] PM200: Wanhua Chemical

[0065] [Examples S1-S6]

[0066] Prepare the raw materials according to the formula in Table 1, keep them warm to 20℃ and mix them evenly. Pour the mixed materials into a 35cm*35cm*10cm foaming mold for foaming. The mold temperature is 38℃ and the feed density is 48kg / m 3 , prepare polyurethane rigid foam.

[0067] Table 1, raw material formula (g) in Examples S1-S6

[0068]

[0069]

[0070] [Comparative Example D1]

[0071] The polyurethane rigid foam was prepared by foaming according to the formula and method basically the same as that in Example S1, except that the polyether polyol A1 was not added and the amount of the polyether polyol D1 was increased accordingly to ensure that the total mass of the combined polyether components remained unchanged.

[0072] [Comparative Example D2]

[0073] The polyurethane rigid foam was prepared by foaming according to the formula and method basically the same as that in Example S1, except that the polyether polyol A1 was replaced by a flame retardant polyol FR212 of the same quality (Wanhua Chemical (Yantai) Rongwei Polyurethane Co., Ltd.).

[0074] The performance tests shown in Table 2 were performed on the polyurethane rigid foams prepared in Examples S1-S6 and Comparative Examples D1-D2, and the test results are as follows. The relevant test methods mainly include:

[0075] (1) Gel time: Wanhua Chemical (Yantai) Rongwei Polyurethane Co., Ltd. Enterprise Standard Q / 0600YPU 026-2022

[0076] (2) Foam core density: Wanhua Chemical (Yantai) Rongwei Polyurethane Co., Ltd. Enterprise Standard Q / 0600YPU 026-2022

[0077] (3) Thermal conductivity: ASTM C518

[0078] (4) Oxygen index: GB / T 2406-009

[0079] (5) Compression strength: GB / T 8813-2008

[0080] (6) Flexural strength: GB / T 8812-2008

[0081] Table 2. Performance test results

[0082]

[0083] From the performance test results of D2 and D1 in Table 2, it can be seen that the introduction of conventional flame-retardant polyether improves the oxygen index to a certain extent, while causing certain damage to the foam strength. It is difficult to improve both at the same time, and it is impossible to fully meet the use requirements of high-strength supporting materials for transport carriers such as refrigerated trucks and refrigerated containers.

[0084] It can be seen from the test results of S1-S6 that the oxygen index of the polyurethane rigid foam obtained by the scheme of the present invention is not only greatly improved by more than 2% compared with D1, which significantly improves the flame retardancy of the foam, but also improves the compression strength and bending strength at the same time, solving the pain points of the industry. The obtained polyurethane rigid foam is particularly suitable for application fields such as refrigerated trucks and refrigerated containers that have high requirements on flame retardancy and foam strength.

[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a flame retardant rigid foam polyether polyol, It is characterized in that The process includes: A silane compound containing a primary amino group and a diphenylphosphonium halide are used as raw materials to react under alkaline conditions to obtain an intermediate; then the intermediate is used as an initiator to undergo a polymerization reaction with an oxidized olefin under the action of a polymerization catalyst to obtain a polyether polyol.

2. The method for preparing the flame retardant rigid foam polyether polyol according to claim 1, It is characterized in that The molar ratio of the silane compound to the diphenylphosphorus halide is 1-3:1; Preferably, the silane compound is selected from one or more of 3-aminopropyltriethoxysilane, (3-aminopropyl)dimethylmethoxysilane, (3-aminoethyl)dimethylmethoxysilane; Preferably, the phenyl phosphorus halide is selected from one or more of diphenyl phosphorus chloride, phenyl phosphorus dichloride, (2-chlorophenyl) diphenylphosphine; Preferably, the alkaline conditions for the reaction of the silane compound and the diphenylphosphonium halide are provided by an organic base and / or an inorganic base; the organic base is selected from one or more of triethylamine, dimethylethylamine, and diisopropylethylamine; the inorganic base is selected from one or more of sodium methoxide, potassium ethoxide, and potassium tert-butoxide; The amount of the organic base and / or inorganic base used is 0.5-2 times the molar amount of the silane compound.

3. The method for preparing the flame retardant rigid foam polyether polyol according to claim 1 or 2, It is characterized in that The olefin oxide is one or more of ethylene oxide, propylene oxide, butylene oxide and tetrahydrofuran; Preferably, the amount of the olefin oxide is 2-8 times the molar amount of the corresponding silane compound; Preferably, the polymerization catalyst is an alkaline catalyst and / or a bimetallic complex catalyst, more preferably one or more of potassium hydroxide, sodium hydroxide, potassium alcoholate, sodium alcoholate, MMC, and DMC; Preferably, the amount of the polymerization catalyst used is 1-3% of the mass of the corresponding silane compound.

4. The method for preparing the flame retardant rigid foam polyether polyol according to any one of claims 1 to 3, It is characterized in that The reaction temperature of the silane compound and the diphenylphosphorus halide is 35-45° C., and the reaction time is 1-3 hours; Preferably, the polymerization reaction is divided into an esterification addition reaction stage and a vacuum aging stage, wherein the esterification addition reaction is a reaction of a silane compound and a polymerization catalyst in a reactor completely replaced with nitrogen, with stirring and heating to 120-150°C, and adding oxidized olefins to react for 1-4 hours; after the esterification addition reaction is completed, the temperature is raised to 180-200°C, and vacuum aging is carried out while maintaining the pressure at no more than 0.8 MPa to evaporate the by-product water and unreacted oxidized olefins.

5. A flame retardant rigid foam polyether polyol prepared by the method according to any one of claims 1 to 4, It is characterized in that The functionality is 1, the hydroxyl value is 70-120 mgKOH / g, and the viscosity at 25°C is 400-800 mPa*s.

6. A flame retardant polyurethane rigid foam, It is characterized in that It comprises a polyisocyanate component and a combined polyether component, wherein the combined polyether component comprises A) a polyol, B) a blowing agent and optionally C) an auxiliary agent; Wherein, A) the polyol comprises a flame retardant rigid foam polyether polyol prepared by the method described in any one of claims 1 to 4; preferably, the mass content of the flame retardant rigid foam polyether polyol prepared by the method described in any one of claims 1 to 4 in A) the polyol is 5 to 40 wt%.

7. The flame retardant polyurethane rigid foam according to claim 6, It is characterized in that The mass ratio of the polyisocyanate component to the combined polyether component is (1-1.5):1; Preferably, the polyisocyanate component is polymeric MDI or liquefied modified MDI, preferably one or more of Wanhua PM200, PM400, and PM700; Preferably, B) the amount of the foaming agent is 5-15% by mass of the combined polyether component; Preferably, the amount of C) the auxiliary agent is 10-20% by weight of the combined polyether component.

8. The flame retardant polyurethane rigid foam according to claim 6 or 7, It is characterized in that A) the polyol optionally further comprises at least one of a polyether polyol with sucrose as an initiator, a polyether polyol with sorbitol as an initiator, a polyether polyol with propylene glycol as an initiator, and a polyester polyol with phthalic anhydride as an initiator; Preferably, the polyether polyol using sucrose as the initiator is a polyether polyol prepared by polymerization of propylene oxide and / or ethylene oxide using sucrose as the initiator, with a molecular weight of 300-800, a functionality of 4.5-6, and a hydroxyl value of 300-420 mgKOH / g; preferably, the mass fraction of the polyether polyol using sucrose as the initiator in A) is ≤40wt%; Preferably, the polyether polyol using sorbitol as the initiator is a polyether polyol prepared by polymerization of propylene oxide and / or ethylene oxide using sorbitol as the initiator, with a molecular weight of 600-700, a functionality of 4.5-6, and a hydroxyl value of 400-500 mgKOH / g; preferably, the mass fraction of the polyether polyol using sorbitol as the initiator in A) is ≤30wt%; Preferably, the polyether polyol with propylene glycol as the initiator is a polyether polyol prepared by polymerization of propylene glycol as the initiator with propylene oxide and / or ethylene oxide, with a molecular weight of 400-1000, a functionality of 1.5-2, and a hydroxyl value of 400-800 mgKOH / g; preferably, the mass fraction of the polyether polyol with propylene glycol as the initiator in A) is ≤30wt%. Preferably, the polyester polyol using phthalic anhydride as the initiator has a molecular weight of 300-500, a functionality of 2, and a hydroxyl value of 220-350 mgKOH / g; preferably, the mass fraction of the polyester polyol using phthalic anhydride as the initiator in A) is ≤20wt%.

9. The flame retardant polyurethane rigid foam according to any one of claims 6 to 8, It is characterized in that The foaming agent is one or more of cyclopentane, isopentane and normal pentane, or a mixture of at least one of cyclopentane, isopentane and normal pentane and water.

10. The flame retardant polyurethane rigid foam according to any one of claims 6 to 9, It is characterized in that The auxiliary agent is one or more of a flame retardant, a surfactant, and a catalyst; Preferably, the flame retardant is tris(chloroisopropyl)phosphate and / or triethyl phosphate; Preferably, the surfactant is a siloxane; Preferably, the catalyst is an amine and / or a metal salt and / or water, more preferably one or more of pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, triethylenediamine, TMR-2, N,N-dimethylbenzylamine, potassium formate, potassium acetate, potassium isooctanoate, and water.

Citation Information

Patent Citations

  • Reactive flame-retardant polyether polyol, polyisocyanurate foam, and preparation method and application of reactive flame-retardant polyether polyol and polyisocyanurate foam

    CN114736364A

  • P-toluenesulfonhydrazide polyether polyol and preparation method thereof as well as flame-retardant polyurethane foam and preparation method thereof

    CN114854002A

  • Polyether polyol as well as preparation method and application thereof

    CN117343313A

  • Diclofenac polyether ester monohydric alcohol, preparation method thereof, flame-retardant polyurethane foam and preparation method thereof

    CN117534828A

Cited By

  • Phosphorus-nitrogen synergistic flame-retardant polyester polyol and preparation method thereof

    CN119331231A

  • Phosphorus-nitrogen synergistic flame-retardant polyester polyol and preparation method thereof

    CN119331231B

  • High-adhesion reactive flame-retardant polyether polyol and preparation method thereof

    CN119331234A

  • Highly adhesive reactive flame-retardant polyether polyol and preparation method thereof

    CN119331234B