Modified silicone oil emulsifier and production process thereof
Through improved process methods, the preparation process of modified silicone oil emulsifier is simplified by utilizing specific raw materials and reaction conditions, reducing reaction temperature and time, and improving the centrifugal stability and hot and cold impactability of the product.
Patent Information
- Application Number
- CN202410968601.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of existing modified silicone oil emulsifiers needs to be carried out under photoinitiators and ultraviolet light, and long-term reactions are required at high temperatures, which increases the difficulty of operation and complexity of reaction conditions.
1,3-dimethyltetramethoxydisiloxane, 1,3-dioxolan-2-one monomer, porous dextran gel and trimethylethoxysilane as raw materials , heat to 55-80°C, react, add hydrochloric acid dropwise and condense and reflux, then mix with hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate, heat to 35-45°C, and finally add chloroplatinic acid dropwise The isopropanol solution was reduced to room temperature to obtain a modified silicone oil emulsifier.
The difficulty and time of reaction conditions are reduced, the reaction efficiency is improved, and the prepared water-in-oil emulsion has high centrifugal stability and good hot and cold impact.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of modified silicone oil preparation, and in particular to a modified silicone oil emulsifier and a production process thereof. Background Art
[0002] Modified silicone oil emulsifiers have the advantages of good emulsification ability, low surface tension, good wetting and spreading effects, defoaming and foam suppression, etc. They are widely used in medical, food, personal care products, electronics and other fields.
[0003] CN109734919A discloses a method for preparing an alkyl / polyether silicone oil emulsifier. The method comprises the following steps: reacting 1,1,3,3-tetramethyl-1,3-divinyldisiloxane and a mercaptan with a general structural formula of HSR, wherein R represents a saturated straight-chain alkyl group of C12-C18, under the irradiation of a photoinitiator and ultraviolet light to obtain an alkyl capping agent; heating octamethylcyclotetrasiloxane, a mercaptopropyl polysiloxane prepolymer and the alkyl capping agent to obtain an alkyl-terminated mercaptopropyl silicone oil; and reacting an alkyl-terminated mercaptopropyl silicone oil, an allyl polyether and an α-unsaturated straight-chain olefin of C12-C20 under the irradiation of a photoinitiator and ultraviolet light to obtain an alkyl / polyether silicone oil emulsifier.
[0004] However, the preparation process requires the reaction under the irradiation of photoinitiator and ultraviolet light (ultraviolet light main wavelength is 365nm, intensity is 80-120W / cm), which increases the difficulty of reaction conditions. At the same time, in the heating reaction, it is necessary to heat up to 110-120℃ for 2 hours, heat up to 140-150℃ for 0.5 hours to destroy the catalyst, reduce the pressure to below -0.09MPa, and remove low-boiling substances for 2 hours. The whole reaction time is long, the temperature is high, and the operation is cumbersome, which further increases the difficulty of reaction conditions.
[0005] Based on this, the present invention designs a modified silicone oil emulsifier and a production process thereof to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a modified silicone oil emulsifier and a production process thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A modified silicone oil emulsifier is prepared by using 1,3-dimethyltetramethoxydisiloxane, 1,3-dioxolane-2-one monomer, porous dextran gel and trimethylethoxysilane as raw materials, heating the mixture to 55-80°C for reaction, dripping hydrochloric acid, condensing and refluxing; then heating the reactants with hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate to 35-45°C for uniform mixing, dripping an isopropanol solution of chloroplatinic acid, and cooling the mixture to room temperature after the dripping is completed, thereby obtaining the modified silicone oil emulsifier.
[0009] Furthermore, the molar ratio of the 1,3-dimethyltetramethoxydisiloxane, the 1,3-dioxolane-2-one monomer, the porous dextran gel and the trimethylethoxysilane is 1: 0.6-0.9: 0.3-0.5: 1.1-1.3.
[0010] Furthermore, the mass ratio of the reactant, hydrogen-containing silicone oil, allyl polyoxyethylene ether, and methyl oleate is 1:0.6-1.1:0.4-0.6:1.2-1.4.
[0011] Furthermore, the dropping speed of the isopropanol solution of chloroplatinic acid is controlled at 25 to 40 drops / min.
[0012] Furthermore, in the isopropanol solution of chloroplatinic acid, the concentration of chloroplatinic acid is 10-15w%.
[0013] Furthermore, hydrochloric acid with a concentration of 15-25w% is added dropwise, and condensed and refluxed for 0.3-0.5h.
[0014] A production process of a modified silicone oil emulsifier comprises the following steps:
[0015] (1) heating the 1,3-dioxolane-2-one monomer and the porous dextran gel to 55-60° C. to react for 0.5-0.8 h to obtain component A;
[0016] (2) heating 1,3-dimethyltetramethoxydisiloxane and trimethylethoxysilane to 70-80° C. to react for 0.8-1 h to obtain component B;
[0017] (3) Component A and component B are mixed, and hydrochloric acid with a concentration of 15 to 25 w% is added dropwise, and condensed and refluxed for 0.3 to 0.5 h to obtain a reactant;
[0018] (4) then heating the reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate to 35-45° C. and mixing them evenly;
[0019] (5) adding an isopropanol solution of chloroplatinic acid dropwise, and cooling the temperature to room temperature to obtain a modified silicone oil emulsifier.
[0020] An emulsifier is used in preparing a water-in-oil emulsion. The oil phase, the water phase and the modified silicone oil emulsifier are weighed, the water phase and the modified silicone oil emulsifier are first mixed evenly, and then slowly added to the oil phase while stirring. After homogenization, the water-in-oil emulsion is obtained.
[0021] Furthermore, homogenization is carried out at a speed of 5000 to 7000 r / min for 10 to 15 minutes.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The invention reduces the difficulty of reaction conditions, and effectively reduces reaction time and temperature; and the water-in-oil emulsion prepared by using the modified silicone oil emulsifier of the invention has the advantages of high centrifugal stability and good thermal shock resistance. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1
[0026] A production process of a modified silicone oil emulsifier comprises the following steps:
[0027] (1) heating 1,3-dioxolane-2-one monomer and porous dextran gel (n1,3-dioxolane-2-one monomer: nporous dextran gel = 0.6:0.5) to 55°C to react for 0.5h to obtain component A;
[0028] (2) heating 1,3-dimethyltetramethoxydisiloxane and trimethylethoxysilane (n1,3-dimethyltetramethoxydisiloxane:ntrimethylethoxysilane=1:1.1) to 80°C to react for 0.8h to obtain component B;
[0029] (3) Component A and component B were mixed, and 15w% hydrochloric acid was added dropwise, and the mixture was condensed and refluxed for 0.3h to obtain a reactant;
[0030] (4) then heating the reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate (m reactants: m hydrogen-containing silicone oil: m allyl polyoxyethylene ether: m methyl oleate = 1:0.6:0.6:1.2) to 45°C and mixing them evenly;
[0031] (5) Add chloroplatinic acid (15w%) in isopropanol solution dropwise (25 drops / min), and cool to room temperature after the addition is complete to obtain a modified silicone oil emulsifier.
[0032] Embodiment 2
[0033] A production process of a modified silicone oil emulsifier comprises the following steps:
[0034] (1) heating 1,3-dioxolane-2-one monomer and porous dextran gel (n1,3-dioxolane-2-one monomer: nporous dextran gel = 0.9:0.3) to 60°C to react for 0.8h to obtain component A;
[0035] (2) heating 1,3-dimethyltetramethoxydisiloxane and trimethylethoxysilane (n1,3-dimethyltetramethoxydisiloxane:ntrimethylethoxysilane=1:1.3) to 70°C to react for 1 hour to obtain component B;
[0036] (3) Component A and component B are mixed, and 25w% hydrochloric acid is added dropwise, and the mixture is condensed and refluxed for 0.5h to obtain a reactant;
[0037] (4) then heating the reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate (m reactants: m hydrogen-containing silicone oil: m allyl polyoxyethylene ether: m methyl oleate = 1:1.1:0.4:1.4) to 35°C and mixing them evenly;
[0038] (5) Add chloroplatinic acid (10w%) in isopropanol solution dropwise (40 drops / min), and cool to room temperature after the addition is complete to obtain a modified silicone oil emulsifier.
[0039] Embodiment 3
[0040] A production process of a modified silicone oil emulsifier comprises the following steps:
[0041] (1) heating 1,3-dioxolane-2-one monomer and porous dextran gel (n1,3-dioxolane-2-one monomer: nporous dextran gel = 0.7:0.4) to 58°C to react for 0.6h to obtain component A;
[0042] (2) heating 1,3-dimethyltetramethoxydisiloxane and trimethylethoxysilane (n1,3-dimethyltetramethoxydisiloxane:ntrimethylethoxysilane=1:1.25) to 76°C to react for 0.7h to obtain component B;
[0043] (3) Component A and component B were mixed, and 18w% hydrochloric acid was added dropwise, and the mixture was condensed and refluxed for 0.4h to obtain a reactant;
[0044] (4) then heating the reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate (m reactants: m hydrogen-containing silicone oil: m allyl polyoxyethylene ether: m methyl oleate = 1: 0.9: 0.5: 1.3) to 38°C and mixing them evenly;
[0045] (5) Add chloroplatinic acid (13w%) in isopropanol solution dropwise (32 drops / min), and cool to room temperature after the addition is complete to obtain a modified silicone oil emulsifier.
[0046] Embodiment 4
[0047] The modified silicone oil emulsifier prepared in Example 3 is used to prepare a water-in-oil emulsion, and the steps are as follows:
[0048] Weigh the oil phase, water phase and modified silicone oil emulsifier, mix the water phase and modified silicone oil emulsifier evenly first, then slowly add them to the oil phase while stirring, and homogenize at a speed of 5000r / min for 10min to obtain an oil-in-water emulsion.
[0049] Embodiment 5
[0050] The modified silicone oil emulsifier prepared in Example 3 is used to prepare a water-in-oil emulsion, and the steps are as follows:
[0051] Weigh the oil phase, water phase and modified silicone oil emulsifier, mix the water phase and modified silicone oil emulsifier evenly, then slowly add them to the oil phase, stirring while adding, homogenize at 7000r / min for 15min to obtain an oil-in-water emulsion. The oil phase uses isododecane.
[0052] The centrifugal stability and thermal shock resistance of the water-in-oil emulsion of Example 5 were tested by the following methods:
[0053] Centrifugal stability: At room temperature, centrifuge the emulsion at 4000 rpm for 20 minutes to observe whether the emulsion is stratified. Result: No stratification.
[0054] Thermal shock: Keep at 40℃ for 30 minutes, cool to -10℃ in 30 minutes, keep for 30 minutes, then heat to 40℃ in 30 minutes, keep for 30 minutes, repeat this cycle 40 times, and observe whether the emulsion is separated. Result: No separation.
[0055] The invention reduces the difficulty of reaction conditions, and effectively reduces reaction time and temperature; and the water-in-oil emulsion prepared by using the modified silicone oil emulsifier of the invention has the advantages of high centrifugal stability and good thermal shock resistance.
[0056] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A modified silicone oil emulsifier, It is characterized in that 1,3-dimethyltetramethoxydisiloxane, 1,3-dioxolane-2-one monomer, porous dextran gel and trimethylethoxysilane are used as raw materials, heated to 55-80°C for reaction, hydrochloric acid is added dropwise, and condensation reflux is performed; then the reactants are heated to 35-45°C and mixed evenly with hydrogenated silicone oil, allyl polyoxyethylene ether and methyl oleate, and an isopropanol solution of chloroplatinic acid is added dropwise. After the addition is completed, the temperature is cooled to room temperature to obtain a modified silicone oil emulsifier.
2. The modified silicone oil emulsifier according to claim 1, It is characterized in that The molar ratio of the 1,3-dimethyltetramethoxydisiloxane, the 1,3-dioxolane-2-one monomer, the porous dextran gel and the trimethylethoxysilane is 1: 0.6-0.9: 0.3-0.5: 1.1-1.
3.
3. The modified silicone oil emulsifier according to claim 2, It is characterized in that The mass ratio of reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate is 1:0.6-1.1:0.4-0.6:1.2-1.
4.
4. The modified silicone oil emulsifier according to claim 3, It is characterized in that The dropping speed of the isopropanol solution of chloroplatinic acid is controlled at 25 to 40 drops / min.
5. The modified silicone oil emulsifier according to claim 4, It is characterized in that In the isopropanol solution of chloroplatinic acid, the concentration of chloroplatinic acid is 10-15w%.
6. The modified silicone oil emulsifier according to claim 5, It is characterized in that Add 15-25w% hydrochloric acid dropwise and condense and reflux for 0.3-0.5h.
7. A production process of the modified silicone oil emulsifier according to claim 6, It is characterized in that The following steps are involved: (1) heating the 1,3-dioxolane-2-one monomer and the porous dextran gel to 55-60° C. to react for 0.5-0.8 h to obtain component A; (2) heating 1,3-dimethyltetramethoxydisiloxane and trimethylethoxysilane to 70-80° C. to react for 0.8-1 h to obtain component B; (3) Component A and component B are mixed, and hydrochloric acid with a concentration of 15 to 25 w% is added dropwise, and condensed and refluxed for 0.3 to 0.5 h to obtain a reactant; (4) then heating the reactants, hydrogen-containing silicone oil, allyl polyoxyethylene ether and methyl oleate to 35-45° C. and mixing them evenly; (5) adding an isopropanol solution of chloroplatinic acid dropwise, and cooling the temperature to room temperature to obtain a modified silicone oil emulsifier.
8. Use of the modified silicone oil emulsifier according to claim 7 in the preparation of a water-in-oil emulsion, It is characterized in that Weigh the oil phase, water phase and modified silicone oil emulsifier, mix the water phase and modified silicone oil emulsifier evenly first, then slowly add them to the oil phase while stirring, and after homogenization, an oil-in-water emulsion is obtained.
9. Use of the emulsifier according to claim 8 in preparing a water-in-oil emulsion, It is characterized in that Homogenize at a speed of 5000-7000 r / min for 10-15 minutes.
Citation Information
Patent Citations
Polyfunctional-group-modified polysiloxane emulsifier and preparation method thereof
CN104177620A
Silicone wax emulsifier
CN106084235A