N-hydroxymethyl methacrylate-formaldehyde-urea copolycondensation resin as well as preparation method and application thereof

Through the preparation method of N-hydroxymethyl methacrylate-formaldehyde-urea co-polycondensed resin, the problems of complex preparation and environmental pollution of traditional resin materials are solved, and resin materials with high reactivity, tunability and environmental protection are achieved. Suitable for a variety of industrial applications.

CN118930872AInactive Publication Date: 2024-11-12SOUTHWEST FORESTRY UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411178377.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation process of traditional resin materials is complex, costly and environmentally polluted, making it difficult to meet the modern industry's demand for excellent performance, low cost and environmental protection.

Method used

The preparation method of N-hydroxymethyl methacrylate-formaldehyde-urea copolycondensation resin is adopted. By prepolymerization, polycondensation and copolycondensation reaction, combined with suitable catalysts and stabilizers, the reaction conditions are controlled to obtain high reaction activity and adjustable Crosslinking density and low formaldehyde-released resin.

Benefits of technology

It significantly improves the adhesion, chemical resistance and weather resistance of the resin, provides adjustable crosslink density and high gloss, is suitable for a variety of application scenarios, reduces the impact on the environment, and meets the requirements of green manufacturing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of new materials, and discloses N-hydroxymethyl methacrylate-formaldehyde-urea copolycondensation resin and a preparation method and application thereof.The method comprises the steps that N-hydroxymethyl methacrylate is dissolved in deionized water, an initiator and a stabilizer are added, a pre-polymerization reaction is conducted, and then the N-hydroxymethyl methacrylate-formaldehyde-urea copolycondensation resin is obtained; adding an initiator to obtain an N-hydroxymethyl methacrylate prepolymer; the preparation method comprises the following steps: dissolving urea in a mixed solution of ethanol and water, dropwise adding a formaldehyde solution, and adding a catalyst I under a stirring condition for reaction to obtain a urea-formaldehyde polycondensate; the N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, a stabilizer I and a catalyst I are added for a reaction, and the N-hydroxymethyl methacrylate-formaldehyde-urea copolycondensation resin is obtained. Through the innovative raw material combination and preparation process, the defects of traditional resin in the aspects of adhesion, weather resistance, environmental protection performance and the like are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to an N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin and a preparation method and application thereof. Background Art

[0002] In modern industry, resin materials are widely used due to their excellent physical and chemical properties. Especially in the fields of coatings, adhesives, composite materials, etc., the demand for resin materials is increasing. Although traditional resin materials such as phenolic resin and epoxy resin have good properties, their preparation process is complicated, the cost is high, and there are certain environmental pollution problems.

[0003] In order to overcome the shortcomings of existing technologies, researchers have been looking for new resin materials and preparation methods. Summary of the invention

[0004] In view of this, the present invention proposes an N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin and a preparation method and application thereof, aiming to provide a new resin material with excellent performance, low cost and environmental friendliness.

[0005] The present invention provides a method for preparing an N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, comprising:

[0006] Dissolving N-hydroxymethyl methacrylate in deionized water, adding an initiator and a stabilizer, and performing a prepolymerization reaction to obtain an N-hydroxymethyl methacrylate prepolymer;

[0007] Dissolve urea in a mixed solution of ethanol and water, add formaldehyde solution dropwise, add catalyst I under stirring to react, and obtain urea-formaldehyde polycondensate;

[0008] The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin.

[0009] Preferably, the initiator is potassium persulfate;

[0010] The stabilizer I is sodium sulfite;

[0011] The catalyst I is ammonium chloride;

[0012] The solvent is dimethyl sulfoxide;

[0013] The stabilizer II is nonylphenol polyoxyethylene ether;

[0014] The catalyst II is aluminum trichloride.

[0015] Preferably, N-hydroxymethyl methacrylate is dissolved in deionized water, an initiator and a stabilizer are added, and a prepolymerization reaction is carried out to obtain an N-hydroxymethyl methacrylate prepolymer at a temperature of 50±2° C. and a pH of 4-5.

[0016] Preferably, urea is dissolved in a mixed solution of ethanol and water, formaldehyde solution is added dropwise, and catalyst I is added under stirring to react to obtain urea-formaldehyde condensation product at a temperature of 60±2° C. and a pH of 3.5-4.5.

[0017] Preferably, urea is dissolved in a mixed solution of ethanol and water, a formaldehyde solution is added dropwise, and a catalyst I is added under stirring to react to obtain a urea-formaldehyde polycondensate, comprising:

[0018] Dissolve urea in a mixed solution of ethanol and water, add formaldehyde solution dropwise, add catalyst I under stirring to react for 1-2 hours, and cool to 5-10° C. after the reaction to obtain urea-formaldehyde polycondensate.

[0019] Preferably, when the N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde condensation product are mixed and dissolved in a solvent, stabilizer II and catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, the mass ratio of the N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde condensation product is 1:1.

[0020] Preferably, the N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and stabilizer II and catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, comprising:

[0021] The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to carry out a co-condensation reaction at 80-90° C., pH 6.0-7.0 and stirring conditions for 4-6 hours to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin.

[0022] Preferably, the N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and stabilizer II and catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, further comprising:

[0023] Sodium hydroxide solution was added dropwise to control the pH value at 6.0-7.0.

[0024] The present invention also provides an N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, and the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin is prepared by the above-mentioned preparation method.

[0025] The present invention also provides an application of the above-mentioned N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, wherein the application comprises at least one of the following:

[0026] A) Application in coatings;

[0027] A) Application in adhesives;

[0028] A) Application in molding materials;

[0029] A) Application in electronic packaging materials;

[0030] A) Application in building materials.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. Enhanced adhesion performance

[0033] The resin combines the high reactivity of N-hydroxymethyl methacrylate with the cross-linking ability of urea-formaldehyde resin, significantly improving adhesion to a variety of substrates. Compared with traditional urea-formaldehyde resin or methacrylate resin, the present invention provides stronger bonding and is suitable for a wider range of application scenarios.

[0034] 2. Adjustable cross-linking density

[0035] The present invention optimizes the reaction conditions and catalyst formula to make the crosslinking density of the resin adjustable, thereby achieving customization for different application requirements without affecting the overall performance of the material. Compared with traditional resins, the present invention can more accurately control key parameters such as hardness, toughness and heat resistance.

[0036] 3.Excellent chemical resistance and weather resistance

[0037] Due to the introduction of N-hydroxymethyl methacrylate, the resin exhibits better chemical corrosion resistance and weather resistance. Compared with the existing urea formaldehyde resin, the present invention still maintains stable performance in harsh environments (such as humidity, high temperature, chemical corrosion), extending the service life of the product.

[0038] 4. High gloss and surface hardness

[0039] The resin of the present invention has excellent surface gloss and hardness after curing, and is suitable for high-end decorative coatings and surface treatment fields. Compared with traditional thermosetting resins, the material can provide better surface effects and improve wear resistance.

[0040] 5. Environmental advantages

[0041] By optimizing the formula and reaction conditions, the resin of the present invention can achieve efficient cross-linking reaction with low formaldehyde release, reducing the impact on the environment. Compared with traditional high formaldehyde content resins, the present invention has better environmental performance and meets the needs of modern green manufacturing.

[0042] 6. Wide application adaptability

[0043] The resin of the present invention has multifunctionality and can be applied to multiple fields such as coatings, adhesives, molding materials, electronic packaging, etc. Compared with the prior art, the present invention provides a high-performance and multi-purpose material selection to meet the specific needs of different industries. DETAILED DESCRIPTION

[0044] The exemplary embodiments of the present disclosure will be described in more detail below. Although the exemplary embodiments of the present disclosure are shown below, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to be able to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0045] Example 1

[0046] 1. Prepolymerization of N-hydroxymethyl methacrylate

[0047] 1. Material preparation

[0048] N-Hydroxymethyl methacrylate;

[0049] Initiator: potassium persulfate (KPS);

[0050] Stabilizer: sodium sulfite;

[0051] Solvent: deionized water.

[0052] 2. Reaction conditions

[0053] At 50°C, N-hydroxymethyl methacrylate was dissolved in deionized water, and potassium persulfate and sodium sulfite were added.

[0054] The pH value of the system was controlled between 4 and 5 to avoid excessive reaction of hydroxymethyl.

[0055] The prepolymerization reaction was carried out under stirring conditions for 2 hours to form a partially polymerized low molecular weight prepolymer.

[0056] After the reaction was completed, the system was cooled to room temperature and the pH value was adjusted to neutral.

[0057] 2. Urea-formaldehyde polycondensation reaction

[0058] 1. Material preparation

[0059] Urea;

[0060] Formaldehyde (37% solution);

[0061] Catalyst: ammonium chloride;

[0062] Solvent: A mixture of ethanol and water.

[0063] 2. Reaction conditions

[0064] Urea was dissolved in a mixed solution of ethanol and water at 60°C, and then the formaldehyde solution was added dropwise.

[0065] Under stirring conditions, a small amount of ammonium chloride is added as an acidic catalyst to control the pH value between 3.5 and 4.5.

[0066] The reaction time is 1-2 hours to form a preliminary urea-formaldehyde polycondensate.

[0067] After the reaction was completed, the mixture was quickly cooled to 8°C to inhibit further polycondensation.

[0068] 3. Co-condensation reaction

[0069] 1. Material preparation

[0070] The N-hydroxymethyl methacrylate prepolymer of step 1;

[0071] The urea-formaldehyde polycondensate of step 2;

[0072] Catalyst: aluminum chloride (AlCl3);

[0073] Stabilizer: nonylphenol polyoxyethylene ether (NP-10);

[0074] Solvent: dimethyl sulfoxide (DMSO).

[0075] 2. Reaction conditions

[0076] At room temperature, N-hydroxymethyl methacrylate prepolymer and urea-formaldehyde polycondensate are mixed in a mass ratio of 1:1, and a small amount of aluminum chloride is added as a catalyst.

[0077] DMSO was used as solvent to increase the mutual solubility of reactants and the reaction rate.

[0078] The temperature was gradually raised to 85° C., and the co-polycondensation reaction was carried out under stirring for 5 hours.

[0079] Nonylphenol polyoxyethylene ether is added as a stabilizer to prevent excessive cross-linking and gelation.

[0080] During the reaction, the viscosity and pH value of the reaction system were closely monitored, and the pH value was controlled between 6.0 and 7.0 by dropping sodium hydroxide solution.

[0081] 4. Post-processing and curing

[0082] After the reaction is completed, the co-condensation reaction mixture is cooled to room temperature, and an appropriate amount of distilled water is gradually added to dilute it to reduce the viscosity of the solution.

[0083] The unreacted residue and insoluble matter were removed by filtration.

[0084] The DMSO solvent was removed by evaporation or rotary evaporator to obtain a solid resin.

[0085] The resin is placed in a mold and subjected to a heat-pressing curing process at 120°C for 2 hours to form a resin material with the final shape and properties.

[0086] 5. Performance Testing

[0087] The heat-cured resin is removed from the mold and cooled to ensure the stability and dimensional accuracy of the resin. It is then cut and polished to obtain the desired shape and surface finish.

[0088] 1. Mechanical properties test

[0089] The cured resin was subjected to tensile, bending and impact tests using a universal material testing machine to evaluate its mechanical strength and toughness. Parameters such as maximum tensile strength, bending strength and impact strength were recorded and compared with standard samples.

[0090] 2. Thermal performance test

[0091] The glass transition temperature (Tg) and thermal stability of the resin were measured using a differential scanning calorimeter (DSC) and a thermogravimetric analyzer (TGA). The thermal behavior of the resin at different temperatures was recorded to evaluate its potential for application in high temperature environments.

[0092] 3. Chemical stability test

[0093] The resin samples are immersed in acid, alkali and organic solvents respectively to observe the changes in mass and surface morphology under different chemical environments. Through these tests, the corrosion resistance and chemical stability of the resin are evaluated.

[0094] 4. Electrical performance test

[0095] Measure the electrical properties of resins such as volume resistivity, surface resistivity and dielectric constant to evaluate their potential applications in the electronic and electrical fields.

[0096] 5. Optical performance test

[0097] For transparent or translucent resin materials, their optical performance parameters such as transmittance, refractive index and dispersion are measured to evaluate their application potential in the optical field.

[0098] Through the above performance tests, we can fully understand the comprehensive performance of resin materials and provide a scientific basis for subsequent application development and product design.

[0099] 6. Test results

[0100] (1) Mechanical properties test results

[0101] After tensile, bending and impact tests, the cured resin showed good mechanical properties. The maximum tensile strength reached 50MPa, the bending strength was 70MPa, and the impact strength was 15kJ / m 2 Compared with the standard samples, all indicators have reached or exceeded the expected requirements, showing excellent mechanical properties.

[0102] (2) Thermal performance test results

[0103] The glass transition temperature (Tg) of the resin was 120°C by DSC and TGA analysis, indicating that it has good heat resistance. Thermogravimetric analysis showed that the mass loss of the resin was less than 5% below 300°C, indicating that it has high thermal stability in high temperature environments.

[0104] (3) Chemical stability test results

[0105] After soaking in acid, alkali and organic solvents for 24 hours, the mass change of the resin was within 1% and there was no obvious change on the surface, indicating that it has good corrosion resistance and chemical stability.

[0106] (4) Electrical performance test results

[0107] The volume resistivity of the resin is 1×10 14 Ω·cm, surface resistivity is 1×10 15 Ω, and the dielectric constant is 3.2. These parameters indicate that the resin has good insulation properties and is suitable for use in electronic and electrical fields.

[0108] (5) Optical performance test results

[0109] For the transparent resin material, its transmittance reaches 90% in the visible light range, the refractive index is 1.5, and the dispersion is small, indicating that it has excellent optical properties and is suitable for application in the optical field.

[0110] In summary, through performance testing, the resin material has excellent mechanical properties, thermal properties, chemical stability, electrical properties and optical properties, and has a wide range of application potential. Based on these test results, the resin formula and preparation process can be further optimized to meet the needs of different fields.

[0111] 6. Principle

[0112] 1. The mechanism of action of sodium sulfite

[0113] Sodium sulfite acts as a reducing agent in the system, which can effectively control the overreaction of hydroxymethyl groups, thereby avoiding undesirable crosslinking reactions. Its reducing property can inhibit the generation of free radicals, thereby stabilizing the progress of the prepolymerization reaction.

[0114] 2. Principle of urea-formaldehyde polycondensation reaction

[0115] Urea and formaldehyde undergo polycondensation under acidic conditions to form urea-formaldehyde resin. Ammonium chloride, as a catalyst, can accelerate the reaction rate while controlling the pH value in the range of 3.5-4.5 to ensure the smooth progress of the reaction. Rapid cooling at a lower temperature can effectively prevent excessive polycondensation, thereby obtaining a prepolymer with an appropriate molecular weight.

[0116] 3. Principle of co-condensation reaction

[0117] N-hydroxymethyl methacrylate prepolymer and urea-formaldehyde polycondensate are catalyzed by aluminum chloride to form a polymer with a complex structure through co-condensation reaction. Dimethyl sulfoxide as a solvent not only improves the solubility of the reactants, but also promotes the uniformity of the reaction. Nonylphenol polyoxyethylene ether as a stabilizer prevents excessive cross-linking and gelation, ensuring the controllability of the reaction.

[0118] 4. Post-processing and curing principles

[0119] After the co-condensation reaction is completed, the pure resin is obtained through dilution, filtration and solvent removal. The hot press curing process further cross-links the resin at high temperature to form a cured material with the final form and properties. During the curing process, the control of temperature and pressure is crucial to the performance of the final product.

[0120] 5. Performance testing principle

[0121] Mechanical performance testing evaluates the strength and toughness of resins by simulating the stress conditions in actual applications. Thermal performance testing evaluates the heat resistance and thermal stability of resins through DSC and TGA analysis. Chemical stability testing evaluates the stability of resins in different chemical environments through immersion experiments. Electrical performance testing evaluates the insulation properties of resins by measuring resistivity and dielectric constant. Optical performance testing evaluates the application potential of resins in the optical field by measuring transmittance and refractive index.

[0122] Through the combined effect of these principles, it can be ensured that the performance of resin materials in different application fields meets the requirements, providing a theoretical basis for product development and application.

[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing an N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, characterized in that: include: Dissolving N-hydroxymethyl methacrylate in deionized water, adding an initiator and a stabilizer, and performing a prepolymerization reaction to obtain an N-hydroxymethyl methacrylate prepolymer; Dissolve urea in a mixed solution of ethanol and water, add formaldehyde solution dropwise, add catalyst I under stirring to react, and obtain urea-formaldehyde polycondensate; The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin.

2. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: The initiator is potassium persulfate; The stabilizer I is sodium sulfite; The catalyst I is ammonium chloride; The solvent is dimethyl sulfoxide; The stabilizer II is nonylphenol polyoxyethylene ether; The catalyst II is aluminum trichloride.

3. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: N-hydroxymethyl methacrylate is dissolved in deionized water, an initiator and a stabilizer are added, and a prepolymerization reaction is carried out to obtain an N-hydroxymethyl methacrylate prepolymer at a temperature of 50±2° C. and a pH of 4-5.

4. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: Urea is dissolved in a mixed solution of ethanol and water, formaldehyde solution is added dropwise, and catalyst I is added under stirring to react to obtain urea-formaldehyde condensation product at a temperature of 60±2° C. and a pH of 3.5-4.

5.

5. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: Dissolving urea in a mixed solution of ethanol and water, adding formaldehyde solution dropwise, adding catalyst I under stirring conditions to react, and obtaining a urea-formaldehyde polycondensate, comprising: Dissolve urea in a mixed solution of ethanol and water, add formaldehyde solution dropwise, add catalyst I under stirring to react for 1-2 hours, and cool to 5-10° C. after the reaction to obtain urea-formaldehyde polycondensate.

6. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, wherein the mass ratio of the N-hydroxymethyl methacrylate prepolymer to the urea-formaldehyde polycondensate is 1:

1.

7. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 1, characterized in that: The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, comprising: The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to carry out a co-condensation reaction at 80-90° C., pH 6.0-7.0 and stirring conditions for 4-6 hours to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin.

8. The method for preparing the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 7, characterized in that: The N-hydroxymethyl methacrylate prepolymer and the urea-formaldehyde polycondensate are mixed and dissolved in a solvent, and a stabilizer II and a catalyst II are added to react to obtain the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin, which further comprises: Sodium hydroxide solution was added dropwise to control the pH value at 6.0-7.

0.

9. An N-hydroxymethyl methacrylate-formaldehyde-urea cocondensation resin, characterized in that: The N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the N-hydroxymethyl methacrylate-formaldehyde-urea co-condensation resin according to claim 9, characterized in that: The application includes at least one of the following: A) Application in coatings; A) Application in adhesives; A) Application in molding materials; A) Application in electronic packaging materials; A) Application in building materials.

Citation Information

Patent Citations

  • Water-dispersible glass fiber coating polymer and preparation method thereof

    CN109942742A

  • Preparation method of urea-formaldehyde water-retention controlled release fertilizer

    CN110128205A

  • Branched polymer-urea-glyoxal copolycondensation resin as well as preparation method and application thereof

    CN113336908A

  • Meshed hyperbranched amino copolycondensation resin as well as preparation method and application thereof

    CN115160520A

  • Preparation method and application of glyoxal-urea-poly (N-hydroxymethyl acrylamide) resin

    CN117946344A