Environment-friendly nano hydrophobic emulsion as well as preparation method and application method thereof

By using the hydrogen-containing siloxane polymer and surfactant, the problems of poor weather resistance and environmental pollution of existing hydrophobic materials are solved, and super hydrophobic effect and long life application is achieved. It is suitable for multiple applications. industry.

CN118930901APending Publication Date: 2024-11-12CEUCOS NANO-COATING TECH (JIAXING L
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411168696.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2017-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing hydrophobic materials have poor weather resistance, short service life, environmental pollution and harmful substances in industrial applications, which limit their large-scale application.

Method used

An environmentally friendly nanohydrophobic emulsion is prepared by using hydrogen-containing siloxane polymers as actives, combined with neutral and anionic surfactants, through specific emulsifier ratios and preparation methods, for modifying inorganic materials to form superhydrophobic surfaces.

Benefits of technology

It has achieved super-heavy, ultra-long life and environmentally friendly nano-heavy effects, and is suitable for construction, agriculture and other fields, reducing costs and improving the weather resistance and safety of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008537810000131
    Figure BDA0005008537810000131
Patent Text Reader

Abstract

The invention relates to the field of hydrophobic materials, in particular to an environment-friendly nano hydrophobic emulsion capable of modifying various inorganic materials into a hydrophobic or partial hydrophobic function as well as a preparation method and an application method of the environment-friendly nano hydrophobic emulsion. The environment-friendly nano hydrophobic emulsion is prepared from the following raw materials in percentage by weight: 1-70% of active matter, 0.1-10% of emulsifier and 98.9-20% of water, wherein the active matter accounts for the total weight of the nano hydrophobic emulsion; the emulsifier accounts for the total weight of the nano hydrophobic emulsion; the emulsifier is composed of a neutral surfactant and an anionic surfactant, and the mixing ratio of the two surfactants is not limited. The environment-friendly nano hydrophobic emulsion has the advantages of being good in weather resistance, free of environmental pollution and free of harmful substances.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the parent application is 201710603859.5, the application date is July 24, 2017, and the name of the invention is “Environmentally friendly nano-hydrophobic emulsion, preparation method and application thereof”. Technical Field

[0002] The invention relates to the field of hydrophobic materials, and in particular to an environmentally friendly nano hydrophobic emulsion capable of modifying various inorganic materials into hydrophobic or partially hydrophobic functions, and a preparation method and an application method thereof. Background Art

[0003] The research and development of nano-hydrophobic technology has developed rapidly in the past 10 years, but there is still a long way to go before it can be suitable for industrial-scale practical application, especially in various inorganic solid materials in nature, such as various soils / clays / silts / stones / sands. There are few practical application technologies in cement / bricks and tiles. There are some products for application in cement / bricks and tiles. At present, these hydrophobic products mainly use long carbon chain silicones as hydrophobic agents, and thus have the following major technical defects: (1) poor weather resistance and short service life, generally 1-3 years; (2) the product contains organic solvents to increase the solubility of silicone in aqueous solution, which not only has high organic volatiles (VOC) and high costs, but more importantly, causes environmental pollution and cannot be applied on an industrial scale; (3) most products contain harmful substances that are harmful to the environment and humans, which also limits large-scale application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an environmentally friendly nano hydrophobic emulsion which has strong hydrophobicity, strong weather resistance, long service life, no harm to humans and the environment, and can be used for large-scale industrial production and construction applications, as well as a preparation method and an application method thereof.

[0005] The environmentally friendly nano hydrophobic emulsion is made of the following raw materials: active substances, emulsifiers, and water; wherein the active substances account for 1-70% of the total weight of the nano hydrophobic emulsion, the emulsifiers account for 0.1-10% of the total weight of the nano hydrophobic emulsion, and the water accounts for 98.9-20% of the total weight of the nano hydrophobic emulsion; in industrial production, the content of the active substances can be any solubility from 1% to 70%, and in actual product application, the content of the active substances in the product depends on the requirements of the application object, and the concentrate can be simply diluted with water in any proportion in the factory or on the construction site.

[0006] The active substance of the nano hydrophobic emulsion is a hydrogen-containing siloxane polymer (also known as hydrogen-containing silicone oil), the hydrogen content of the active substance of the nano hydrophobic emulsion is 0.1%-1.7%, and the molecular formula of the hydrogen-containing siloxane polymer is:

[0007] (R)3SiO[RHSiO] nSi(R)3, R = alkyl with 1 to 5 carbon atoms;

[0008] The emulsifier is composed of a neutral surfactant and an anionic surfactant, and the mixing ratio of the two types of surfactants is not limited;

[0009] The neutral surfactant may be a fatty alcohol, ether, or ester compound, or a mixture thereof, and the mixing ratio is not limited;

[0010] The anionic surfactant is a fatty sulfate or a fatty sulfonate or a fatty acid salt, or a mixture thereof, and the mixing ratio is not limited;

[0011] The fatty alcohols can be: saturated or unsaturated alkanes containing at least one or more alcoholic hydroxyl groups (-OH) and 6-30 straight-chain or branched carbons, and can also contain 0-3 carboxyl (-COO-) derivatives, such as lauryl alcohol, stearyl alcohol and palmityl alcohol.

[0012] The ethers can be: saturated or unsaturated alkanes containing at least one or more ether groups (COC) and at least two straight or branched carbons with 6-30 carbon atoms, or derivatives of polyethylene glycol, HO[CH2CH2O] n -H (n = 100-100000), such as laureth, peregal-10, polyethylene glycol 1000, HO[CH2CH2O] 1000 -H.

[0013] The ester compound can be: a saturated or unsaturated fatty acid derivative (-COOC-) containing 6-30 straight-chain or branched carbons, and can also contain 0-5 alcohol hydroxyl groups, such as distearic acid glyceryl, monostearic acid glyceryl, etc.

[0014] The fatty acid or its salt can be: a saturated or unsaturated fatty acid (-COOH) or a fatty acid salt (-COOM, M = Na, K, Ca, etc.) containing 6-30 straight-chain or branched carbon atoms, or a fatty acid sulfate (ROSO 3- ), or fatty sulfonates (RSO3 - ), such as oleic acid, sodium laurate, sodium lauryl sulfate and sodium dodecyl sulfate.

[0015] The preparation method of the nano hydrophobic emulsion:

[0016] Dissolve the emulsifier in 50-80℃ hot water in proportion, stir the mixture mechanically for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to about 25℃ at room temperature, adjust the pH value to 7±1 with a small amount of 10% hydrochloric acid or 10% sodium hydroxide solution; then stir the emulsion with a high shear machine at 800 to 2000rpm, and slowly add the active substance. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform milky concentrated emulsion is formed. When used, the concentrate can be simply diluted with water in any proportion to prepare a nano hydrophobic dilution emulsion suitable for different applications.

[0017] Application method of the nano hydrophobic emulsion:

[0018] Nano hydrophobic emulsions can be mixed with liquid, semi-solid or solid materials for application. For example, they can be mixed with concrete to build cement facilities that are hydrophobic inside and outside, mixed with soil / stone / sand to build dirt roads or earth roadbeds or other dirt facilities that are hydrophobic inside and outside, and can also be mixed with building coatings, unburned brick materials, clay / stone / sand, etc. to prepare hydrophobic materials for various different needs.

[0019] Application areas of nano-hydrophobic emulsions: (1) Construction industry, water conservancy facilities, roads / airports / docks / bridges / roadbeds, etc., application materials include cement / bricks / stones / paints / soil / gypsum, etc.; (2) Agriculture / forestry / animal husbandry / plantations / resorts / ecological parks, etc., application methods include building low-cost, environmentally friendly, and original ecological hydrophobic soil roads, soil squares or parking lots and soil facilities / soil buildings, hydrophobic soil reservoirs or canals, etc.; (3) Soil modification of soil land that is not suitable for planting, such as clay, to improve it into a benign soil that is beneficial to crop growth and moisture retention.

[0020] The dosage of nano hydrophobic emulsion in application: the active matter in the nano hydrophobic emulsion is 0.05% to 2% of the weight of materials such as mud / soil, concrete, building coatings, mortar, etc.

[0021] Construction method of hydrophobic cement-soil highway using nano-hydrophobic emulsion:

[0022] Surface hydrophobicity: Nano hydrophobic emulsion can be directly applied on the solid surface of inorganic materials. The construction methods include painting, spraying, soaking, or wetting.

[0023] Internal and external hydrophobicity (concrete, soil, paint): Nano hydrophobic emulsion can be directly mixed with concrete, soil or sand and stone, architectural coatings, etc. in a certain proportion (the active matter in the hydrophobic material is 0.05% to 2% of the weight of concrete, etc.) to build cement facilities with internal and external hydrophobicity, dirt roads, dirt roadbeds instead of stones, dirt facilities, modified or controllable hydrophobicity of clay, hydrophobic coatings, etc.

[0024] Methods of constructing a sewerage soil road or roadbed:

[0025] (1) Use road construction machinery to loosen the top 5-50 cm thick soil of the dirt road;

[0026] (2) spraying a nano hydrophobic emulsion on loose dry soil, wherein the active substance in the nano hydrophobic emulsion is 0.05% to 2% of the weight of the dry soil;

[0027] (3) using a road construction machine such as a grader or a tiller to uniformly mix the soil and the nano-hydrophobic emulsion, and mixing 90% of the soil into particles with a diameter of about 1 mm to 5 cm;

[0028] Alternatively, other machinery may be used to complete the above steps (2) and (3) in one step with a set of machinery, that is, the soil sprayed with the emulsion may be stirred by the same machinery while spraying the emulsion, so that the spraying and mixing are completed at one time.

[0029] (4) Use a grader or other machinery to make the mixed soil into an arched road surface according to the road construction method, and drainage facilities such as drainage ditches should be installed on both sides of the road;

[0030] (5) A road roller or compactor is used to repeatedly press the road surface until a hard and smooth road surface is formed;

[0031] (6) The wet dirt road needs a 2-10 day incubation and drying period until it forms a dry and hard porous dirt road. The incubation and drying time depend on the temperature and humidity of the environment. Generally, the ambient temperature should be above 20 degrees.

[0032] The above steps (1) to (6) can also be used as a roadbed for building asphalt roads or cement roads, replacing stone roadbeds.

[0033] After it is completely dry, a hydrophobic soil road is formed. Tests such as pouring water or raining confirm that water flows away from the road surface and cannot penetrate and soak the dirt road. The road surface remains hard and dry, and can generally carry 5-15 tons of trucks (the load capacity depends on the soil quality and construction technology. Improved methods can reach a load capacity of more than 50 tons). The road surface forms a hydrophobic surface or even a super hydrophobic surface.

[0034] Construction and application method of clay with controlled hydrophobic strength:

[0035] The method of using nano-hydrophobic emulsion to treat soil, especially clay, with controllable hydrophobic intensity (or moderate hydrophobic intensity treatment) is:

[0036] (1) Use machinery such as an agricultural tiller to loosen the soil to a depth of 5-30 cm;

[0037] (2) spraying the nano-hydrophobic emulsion evenly on the loose soil according to the experimental proportion, wherein the active substance in the nano-hydrophobic emulsion is 0.05% to 2% of the weight of the soil;

[0038] (3) Use a tiller to evenly mix and stir the soil and the sprayed nano-hydrophobic emulsion several times, and stir 90% of the soil into particles with a diameter of about 0.2 cm to 5 cm; or use other tillers to complete steps (2) and (3) at the same time, that is, spray the hydrophobic material while stirring the soil sprayed with the hydrophobic material with the same tiller, so that the spraying and mixing are completed at one time.

[0039] Dry in a natural environment for 2-10 days, and then you can start farming when the treated soil is basically dry.

[0040] The advantages of the present invention are:

[0041] Super hydrophobic, super stable: Compared with existing hydrophobic technologies and products, the nano-hydrophobic emulsion and products of the present invention form better hydrophobic effects on the surfaces of natural inorganic materials such as cement, bricks and tiles, soil, gypsum, etc., and can achieve super hydrophobic effects (hydrophobic angle greater than 150 degrees). The nano-hydrophobic materials formed have better weather resistance and further extend their service life (up to 10 years), which is much longer than the 2-3 years results of our testing of existing market products.

[0042] The hydrogen-containing siloxane polymer in the present invention reacts with polar hydroxyl groups on the porous solid surface, thereby removing the hydrophilic hydroxyl groups and firmly bonding the non-polar hydrophobic organosilicon to the solid surface, and forming nano-scale porous silicon particles, which have the function and characteristics of forming super-hydrophobicity, so the hydrogen-containing siloxane polymer (hydrogen-containing silicone oil) in the present invention forms a stronger and more stable hydrophobic surface than the commonly used single-molecule carbon chain silane (carbon chain length is 1-30). The hydrophobic material of the present invention can form a super-hydrophobic effect on the solid surface of cement / brick / sand / soil / gypsum, so it has a stronger protective effect and self-cleaning function, and the porous silicon particles formed have stronger weather resistance and longer service life, and the amount applied is relatively less, and the application cost is relatively lower.

[0043] Completely environmentally friendly and safe: it does not contain any organic solvents and volatile or flammable organic matter, the volatile organic matter (VOC) is less than 3% (far lower than the national standard of 20% for indoor paints), does not contain any toxic and harmful substances, and can be used in large-scale industrial construction. Its products and industrial applications are safe and harmless to humans, animals, plants and the environment.

[0044] Wide range of applications: Suitable for any building materials such as concrete, cement facilities, brick and tile buildings, earth facilities, coatings and gypsum.

[0045] Energy saving and low cost: The raw materials used to build cement roads and asphalt roads are high-cost, high-energy-consuming and environmentally polluting products. The raw materials used in the present invention have the characteristics of low cost, low energy consumption, safety and environmental protection.

[0046] Soil improvement for farming: Use this nano-hydrophobic emulsion to treat the soil, especially clay, with controllable hydrophobic intensity (or moderate hydrophobic intensity treatment) to reduce its viscosity, so as to improve the soil that is not conducive to crop growth or has poor moisture retention into a benign soil that is beneficial to plant growth and has increased moisture retention performance. DETAILED DESCRIPTION

[0047] The environmentally friendly nano hydrophobic emulsion is made of the following raw materials: active substances, emulsifiers, and water; wherein the active substances account for 1%-70% of the total weight of the nano hydrophobic emulsion, the emulsifier accounts for 0.1%-10% of the total weight of the nano hydrophobic emulsion, and the water accounts for 98.9%-20% of the total weight of the nano hydrophobic emulsion;

[0048] The active substance of the nano hydrophobic emulsion is a hydrogen-containing siloxane polymer (also known as hydrogen-containing silicone oil), the hydrogen content of the active substance of the nano hydrophobic emulsion is 0.1%-1.7%, and the molecular formula of the hydrogen-containing siloxane polymer is:

[0049] (R)3SiO[RHSiO] n Si(R)3, R = alkyl with 1 to 5 carbon atoms;

[0050] The emulsifier is composed of a neutral surfactant and an anionic surfactant, and the mixing ratio of the two types of surfactants is not limited;

[0051] The neutral surfactant may be a fatty alcohol, ether, or ester compound, or a mixture thereof, and the mixing ratio is not limited;

[0052] The anionic surfactant is a fatty sulfate or a fatty sulfonate or a fatty acid salt, or a mixture thereof, and the mixing ratio is not limited;

[0053] The fatty alcohols can be: saturated or unsaturated alkanes containing at least one or more alcoholic hydroxyl groups (-OH) and 6-30 straight-chain or branched carbons, and can also contain 0-3 carboxyl (-COO-) derivatives, such as lauryl alcohol, stearyl alcohol and palmityl alcohol.

[0054] The ethers can be: saturated or unsaturated alkanes containing at least one or more ether groups (COC) and at least two straight or branched carbons with 6-30 carbon atoms, or derivatives of polyethylene glycol, HO[CH2CH2O] n -H (n = 100-100000), such as laureth, peregal-10, polyethylene glycol 1000, HO[CH2CH2O]1000 -H.

[0055] The ester compound can be: a saturated or unsaturated fatty acid derivative (-COOC-) containing 6-30 straight-chain or branched carbons, and can also contain 0-5 alcohol hydroxyl groups, such as distearic acid glyceryl, monostearic acid glyceryl, etc.

[0056] The fatty acid or its salt can be: a saturated or unsaturated fatty acid (-COOH) or a fatty acid salt (-COOM, M = Na, K, Ca, etc.) containing 6-30 straight-chain or branched carbon atoms, or a fatty acid sulfate (ROSO3 - ), or fatty sulfonates (RSO3 - ), such as oleic acid, sodium laurate, sodium lauryl sulfate and sodium dodecyl sulfate.

[0057] The preparation method of the nano hydrophobic emulsion:

[0058] Dissolve the emulsifier in 50-80℃ hot water in proportion, stir the mixture mechanically for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to about 25℃ at room temperature, adjust the pH value to 7±1 with a small amount of 10% hydrochloric acid or 10% sodium hydroxide solution; then stir the emulsion with a high shear machine at 800 to 2000rpm, and slowly add the active substance. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform milky concentrated emulsion is formed. When used, the concentrate can be simply diluted with water in any proportion to prepare a nano hydrophobic dilution emulsion suitable for different applications.

[0059] Application method of the nano hydrophobic emulsion:

[0060] First, the nano-hydrophobic emulsion can be directly applied to the solid surface to be protected, such as cement / brick / gypsum board / soil / stone, etc. The construction methods include brushing, spraying, soaking, etc.

[0061] Second, the nano-hydrophobic emulsion can be mixed with liquid, semi-solid or solid materials for application. For example, it can be mixed with concrete to build cement facilities that are hydrophobic inside and outside, mixed with soil / stone / sand to build dirt roads or earth roadbeds or other dirt facilities that are hydrophobic inside and outside, and can also be mixed with building coatings, unburned brick materials, clay / stone / sand, etc. to prepare hydrophobic materials with different needs.

[0062] Application areas of nano-hydrophobic emulsions: (1) Construction industry, water conservancy facilities, roads / airports / docks / bridges / roadbeds, etc., application materials include cement / bricks / stones / paints / soil / gypsum, etc.; (2) Agriculture / forestry / animal husbandry / plantations / resorts / ecological parks, etc., application methods include building low-cost, environmentally friendly, and original ecological hydrophobic soil roads, soil squares or parking lots and soil facilities / soil buildings, hydrophobic soil reservoirs or canals, etc.; (3) Soil modification of soil land that is not suitable for planting, such as clay, to improve it into a benign soil that is beneficial to crop growth and moisture retention.

[0063] The dosage of nano hydrophobic emulsion in application: the active matter in the hydrophobic material is 0.05% to 2% of the weight of the material such as mud / soil, concrete, architectural coatings, mortar, etc.

[0064] Construction method of hydrophobic cement-soil highway using nano-hydrophobic emulsion:

[0065] Surface hydrophobicity: Nano hydrophobic emulsion can be directly applied on the solid surface of inorganic materials. The construction methods include painting, spraying, soaking, or wetting.

[0066] Internal and external hydrophobicity (concrete, soil, paint): Nano hydrophobic emulsion can be directly mixed with concrete, soil or sand and stone, architectural coatings, etc. in a certain proportion (the active matter in the hydrophobic material is 0.05% to 2% of the weight of concrete, etc.) to build cement facilities with internal and external hydrophobicity, dirt roads, dirt roadbeds instead of stones, dirt facilities, modified or controllable hydrophobicity of clay, hydrophobic coatings, etc.

[0067] Methods of constructing a sewerage soil road or roadbed:

[0068] (1) Use road construction machinery to loosen the top 5-50 cm thick soil of the dirt road;

[0069] (2) spraying a nano hydrophobic emulsion on loose dry soil, wherein the active substance in the hydrophobic material is 0.05% to 2% of the weight of the dry soil;

[0070] (3) using a road construction machine such as a grader or a tiller to uniformly mix the soil and the nano-hydrophobic emulsion, and mixing 90% of the soil into particles with a diameter of about 1 mm to 5 cm;

[0071] Alternatively, other machinery may be used to complete the above steps (2) and (3) in one step with a set of machinery, that is, the soil sprayed with the emulsion may be stirred by the same machinery while spraying the emulsion, so that the spraying and mixing are completed at one time.

[0072] (4) Use a grader or other machinery to make the mixed soil into an arched road surface according to the road construction method, and drainage facilities such as drainage ditches should be installed on both sides of the road;

[0073] (5) A road roller or compactor is used to repeatedly press the road surface until a hard and smooth road surface is formed;

[0074] (6) The wet dirt road needs a 2-10 day incubation and drying period until it forms a dry and hard porous dirt road. The incubation and drying time depend on the temperature and humidity of the environment. Generally, the ambient temperature should be above 20 degrees.

[0075] The above steps (1) to (6) can also be used as a roadbed for building asphalt roads or cement roads, replacing stone roadbeds.

[0076] After it is completely dry, a hydrophobic soil road is formed. Tests such as pouring water or raining confirm that water flows away from the road surface and cannot penetrate the wet soil road. The road surface remains hard and dry. It can generally carry 5-15 tons of trucks (the load capacity depends on the soil quality and construction technology. With improved methods, the load capacity can reach more than 50 tons). The road surface forms a hydrophobic surface or even a super hydrophobic surface.

[0077] Construction and application method of clay with controlled hydrophobic strength:

[0078] The method of using hydrophobic materials to treat soil, especially clay, with controllable hydrophobic strength (or moderate hydrophobic strength treatment) is:

[0079] (1) Use machinery such as an agricultural tiller to loosen the soil to a depth of 5-30 cm;

[0080] (2) spraying the nano-hydrophobic emulsion evenly on the loose soil according to the experimental proportion, wherein the active substance in the nano-hydrophobic emulsion is 0.05% to 2% of the weight of the soil;

[0081] (3) Use a tiller to evenly mix the soil and the sprayed liquid several times, and stir 90% of the soil into particles with a diameter of about 0.2 cm to 5 cm;

[0082] Alternatively, other tilling machines may be used to complete the above steps (2) and (3) at one time, that is, the emulsion is sprayed while the soil sprayed with the hydrophobic material is stirred with the tilling machine at the same time, so that the spraying and mixing are completed at one time.

[0083] Dry in a natural environment for 2-10 days, and then you can start farming when the treated soil is basically dry. DETAILED DESCRIPTION

[0085] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0086] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0087] Example 1

[0088] Take 7 grams of lauryl alcohol, 8 grams of peregal-10, 20 grams of lauric acid (sodium laurate), and 8 grams of sodium lauryl sulfate and dissolve them in 567 grams of 60°C water, and adjust the pH value to 7±1 with a small amount of 10% hydrochloric acid solution. Mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to room temperature of about 25°C; stir the emulsion at a speed of 1200rpm with a high shear machine, and slowly add 390 grams of hydrogenated silicone oil. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform 39% milky white concentrated emulsion is formed.

[0089] Embodiment 2:

[0090] In a 1.5-ton emulsifying tank, add 786 kg of water, then add 7 kg of sodium laurate, 5 kg of sodium lauryl sulfate and 2 kg of stearyl alcohol, heat to 70 degrees, and mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; then cool the emulsion until the temperature drops to room temperature around 25°C, and adjust the pH value to 7±1 with a small amount of 10% hydrochloric acid solution; stir the emulsion at a speed of 1500 rpm with a high shear machine, and slowly add 200 kg of hydrogenated silicone oil. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform 20% milky white concentrated emulsion is formed.

[0091] Embodiment 3:

[0092] Take 14 grams of lauryl alcohol, 19 grams of peregal-10, 51 grams of oleic acid, and 16 grams of sodium lauryl sulfate and dissolve them in 1500 grams of 60°C water, and adjust the pH value to 7±1 with a small amount of 10% sodium hydroxide solution, and mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to room temperature of about 25°C; stir the emulsion at a speed of 1200rpm with a high shear machine, and slowly add 1000 grams of hydrogen-containing silicone oil. After the addition, continue to stir the mixture at a high speed for 30 minutes until a uniform milky white emulsion is formed, continue to stir the emulsion, and add 97.4 kilograms of water to prepare a 1% diluted emulsion.

[0093] Embodiment 4:

[0094] Take 6 grams of palmityl alcohol, 10 grams of lauryl alcohol, 54 grams of oleic acid, and 30 grams of sodium dodecyl sulfate and dissolve them in 200 grams of 85°C water. Mechanically stir the mixture for 30 minutes until a uniform viscous emulsion is formed; when the emulsion temperature drops to about 60°C, adjust the pH value to 7±1 with a small amount of 10% sodium hydroxide solution; stir the emulsion with a high shear machine at a speed of 800-1000rpm, and slowly add 700 grams of hydrogenated silicone oil at the same time. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform 70% milky white highly concentrated emulsion is formed.

[0095] Embodiment 5:

[0096] Take 5 grams of distearin, 8 grams of sodium lauryl sulfate, 7 grams of laureth, 38 grams of oleic acid, and 6 grams of peregal-10 and dissolve them in 286 grams of 85°C water, and mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to about 60°C, adjust the pH value to 7±1 with a small amount of 10% sodium hydroxide solution; stir the emulsion with a high shear machine at a speed of 800 to 1000 rpm, and slowly add 650 grams of hydrogenated silicone oil at the same time. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform 65% milky white concentrated emulsion is formed.

[0097] Embodiment 6:

[0098] In a 1.5-ton emulsifying tank, add 498 kg of water, then add 9 kg of laureth, 7 kg of glyceryl monostearate, 32 kg of oleic acid, and 4 kg of sodium dodecyl sulfate, heat to 70 degrees, and mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; then cool the emulsion until the temperature drops to about 40°C, and adjust the pH value to 7±1 with a small amount of 10% sodium hydroxide solution; stir the emulsion with a high shear machine at a speed of 1200 rpm, and slowly add 500 kg of hydrogenated silicone oil. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform 50% milky white concentrated emulsion is formed.

[0099] Preparation and detection of cement surface hydrophobicity:

[0100] According to the national standard JC / T 902-2002, 10 standard cement blocks (75mm×25mm×15mm) were prepared and treated with the diluted emulsion of nano-hydrophobic emulsion according to the method of the standard. After complete drying, the test results are as follows:

[0101]

[0102] * National paint standard "GB18582-2001 Limits of harmful substances in interior wall paints for interior decoration materials"

[0103] Embodiment 7:

[0104] Mixing with concrete to prepare cement with super hydrophobic inside and outside and method thereof: 500 grams of standard concrete and 2000 grams of fine sand are fully mixed, 100 grams of 50% nano-hydrophobic material and 200 grams of water are fully mixed and added to the mixed concrete / sand, and stirred continuously until uniform, and then put into a mold, vibrate the mold with a hammer for about 10 times around the mold, scrape the surface with a scraper at an angle of 10-20 degrees, place it at room temperature of about 23 degrees for 15 hours, then demould, place it in water at room temperature for 15 days, and take it out and dry it for 5-10 days. After the prepared cement sample block is completely dried, a hydrophobic test is carried out, and both the internal hydrophobicity and the external hydrophobicity of the cement form a super hydrophobic effect.

[0105] Example 8, preparation of cement with weak internal and external hydrophobicity by mixing with concrete and method thereof: 500 grams of standard concrete and 2000 grams of fine sand are fully mixed, 3 grams of 50% nano-hydrophobic material and 297 grams of water are fully mixed and added to the mixed concrete / sand, and stirred continuously until uniform, and then put into a mold, vibrate the mold with a hammer for about 10 times around the mold, scrape the surface with a scraper at an angle of 10-20 degrees, place it at room temperature of about 23 degrees for 24 hours, then demold, place it in water at room temperature for 15 days, and take it out and dry it for 5-10 days. The prepared cement sample block is completely dried and subjected to a hydrophobic test, showing a weak hydrophobic effect.

[0106] Example 9, preparation of cement with super hydrophobicity inside and outside by mixing with concrete and method thereof: 500 grams of standard concrete and 2000 grams of fine sand are fully mixed, 25 grams of 50% nano-hydrophobic material and 275 grams of water are fully mixed and added to the mixed concrete / sand, and stirred continuously until uniform, and then put into a mold, vibrate the mold with a hammer for about 10 times around the mold, scrape the surface with a scraper at an angle of 10-20 degrees, place it at room temperature of about 23 degrees for 20 hours, then demould, place it in water at room temperature for 15 days, and take it out and dry it for 5-10 days. The prepared cement sample block is completely dried and then subjected to hydrophobicity test, and both the hydrophobicity of the cement inside and outside is better than the above experimental results.

[0107] Example 10, preparation method of hydrophobic soil and soaking and water absorption experiment:

[0108] 700 grams of dry red clay is put into a container and crushed to make it loose. 50 grams of 50% concentrated hydrophobic emulsion is mixed with 40 grams of water to make 90 grams of nano-hydrophobic diluted emulsion. The prepared diluted liquid is poured into the loose red clay and stirred with a stirring rod to form semi-solid mud. Square samples are made and dried at 40 to 80 degrees for 24 hours until completely dry. Then, they are placed at 25-40 degrees for 10 days to form good hydrophobic mud.

[0109] Example 11, preparation method of weak hydrophobic soil:

[0110] 700 grams of dry red clay is put into a container and crushed to make it loose. 2.5 grams of 50% concentrated hydrophobic emulsion is mixed with 87.5 grams of water to prepare 90 grams of nano-hydrophobic diluted emulsion. The prepared diluted liquid is poured into the loose red clay and stirred with a stirring rod to form semi-solid mud. A square sample is made and placed at a temperature of 20-50 degrees for 10 days to form weakly hydrophobic mud.

[0111] Example 12, preparation method of super-phobic cement and soaking and water absorption experiment:

[0112] 700 grams of dry red clay is put into a container and crushed to make it loose. 100 grams of 50% concentrated hydrophobic emulsion is poured into the loose red clay and stirred with a stirring rod to form semi-solid mud. A square sample is made and placed at a temperature of 20-50 degrees for 5-10 days to form super-hydrophobic mud inside and outside.

[0113] Determination of water absorption rate of hydrophobic soil: Prepare 5 hydrophobic soil samples, measure and record the total area and dry weight of each sample, then put the 5 samples into 25-degree water, the depth from the liquid surface to the upper surface of the sample is 10 cm, and let it stand for 24 hours. The samples do not change in the water, and the surface is still hard like dry soil, without soil falling off or mud forming. Take it out of the water after 24 hours, wipe the surface with dry cloth or paper, and there is no obvious trace of soil on the cloth or paper after wiping. Weigh the dried samples immediately. The weight difference of each sample and its area ratio are the water absorption rate of the sample. The average water absorption rate of these 5 samples is 442 g / m2.

[0114] Embodiment 13, construction method of building drainage cement soil road:

[0115] In the first step, the dry dirt road was loosened to 15 cm deep, 6 m wide and 100 m long using an excavator and a grader;

[0116] In the second step, 9.5 tons of nano-hydrophobic dilution emulsion is prepared by mixing 0.96 tons of 50% concentrated hydrophobic emulsion with 8.54 tons of water to prepare 9.5 tons of nano-hydrophobic dilution emulsion, and 9.5 tons of nano-hydrophobic dilution emulsion is evenly sprayed on the loose soil.

[0117] The third step is to use an agricultural tiller or land grader to mix the soil and liquid thoroughly and evenly 3-5 times;

[0118] The fourth step is to use a grader to make the mixed soil into an arched road surface according to the road construction method, and drainage facilities should be installed on both sides of the road;

[0119] In the fifth step, a heavy-duty road roller repeatedly presses the road surface until a hard and smooth road surface is formed;

[0120] Step 6: After the wet dirt road is dried for 10-2 days in dry weather with an ambient temperature of 15-40 degrees, the surface has become a dry and hard hydrophobic soil road surface. The experiment of simulating heavy rain confirmed that rainwater cannot penetrate the wet hydrophobic soil road surface and can easily flow away from the road surface. After the rain, the road surface remains hard and intact without forming mud. 8-15 tons of trucks repeatedly drive on the hydrophobic soil road surface in and after the rain. The road surface that the wheels have rolled over remains hard and intact, with no signs of damage, no mud, and the tire surface remains clean without obvious mud.

[0121] Embodiment 14, construction method of building cheap water-repellent cement soil road:

[0122] In the first step, the dry dirt road was loosened mechanically to a depth of 15 cm, 3 m wide and 10 m long;

[0123] In the second step, 45 kg of nano diluted emulsion is prepared by mixing 5.7 kg of 50% concentrated hydrophobic emulsion with 39.3 kg of water to prepare 45 kg of nano hydrophobic diluted emulsion, and 45 kg of nano hydrophobic diluted emulsion is evenly sprayed on the loose soil.

[0124] The third step is to use a small machine to mix the soil and liquid thoroughly and evenly 3-5 times;

[0125] The fourth step is to make the mixed soil into an arched road surface according to the road construction method;

[0126] In the fifth step, the road roller repeatedly presses the road surface until a hard and smooth road surface is formed;

[0127] Step 6: After the wet dirt road is dried for 10-3 days in dry weather with an ambient temperature of 15-40 degrees, the surface has formed a dry and hard weak hydrophobic cement soil road surface. The simulation of heavy rain experiments confirmed that it is difficult for rainwater to penetrate the weak hydrophobic cement soil road surface, and the road surface remains intact after rain.

[0128] Example 15, construction method for building a super-drainable cement soil road:

[0129] In the first step, the dry dirt road was loosened mechanically to a depth of 15 cm, 3 m wide and 10 m long;

[0130] The second step is to evenly spray 187 kg of 60% nano hydrophobic emulsion on the loose soil.

[0131] The third step is to use a small machine to mix the soil and liquid thoroughly and evenly for 3-5 times to form a muddy state;

[0132] The fourth step is to make the mixed mud into an arched road surface according to the road construction method, and then dry it naturally for 1-3 days. When the surface becomes harder, use a roller to roll the road;

[0133] In the fifth step, the road roller repeatedly presses the road surface until a hard and smooth road surface is formed;

[0134] The sixth step is to continue drying the wet dirt road for 10-2 days in dry weather with an ambient temperature of 15-40 degrees, and the surface will form a dry and hard super-hydrophobic cement soil road surface.

[0135] Example 16, implementation method of clay modification:

[0136] Two portions of 10 kg each of red clay were prepared, one portion A was used as a control experiment, and the other portion B was subjected to a weak hydrophobic treatment.

[0137] First, prepare 0.75 kg of nano diluted emulsion, mix 0.15 kg of 20% concentrated hydrophobic emulsion with 0.6 kg of water to prepare 0.75 kg of nano hydrophobic diluted emulsion. Fully mix and stir 10 kg of dry clay B with 0.75 kg of nano hydrophobic diluted emulsion, all dry soil is moistened by the emulsion, and 90% of the wet soil blocks or particles formed have a diameter of 0.1 cm to 2 cm, and then dry naturally at an ambient temperature of 20-40 degrees, and continue to dry for 5-10 days. At this time, clay B has shown weak hydrophobic characteristics.

[0138] Clay samples A and B were placed in two containers, and 3 kg of water was sprayed on each sample. Clay A was completely wet and absorbed all the water, while the particles of clay B were semi-wet, and some water naturally flowed into the soil from the gaps between the particles. Stirring A and B separately, clay A became muddy, while clay B did not form the mud phenomenon like clay A. After samples A and B were placed for several days until they were dry, sample A formed a large hard soil block with large cracks, which was difficult to break, while sample B formed smaller cracks and smaller soil blocks. Due to the reduced viscosity, it was loose and easier to break into particles. After the water spray test, the viscosity of the partially hydrophobic clay was significantly weakened.

[0139] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. An environmentally friendly nano hydrophobic emulsion, characterized by: The invention is prepared from the following raw materials: active substance, emulsifier and water; wherein the active substance accounts for 1-70% of the total weight of the nano hydrophobic emulsion, the emulsifier accounts for 0.1-10% of the total weight of the nano hydrophobic emulsion, and the water accounts for 98.9-20% of the total weight of the nano hydrophobic emulsion; The emulsifier is composed of a neutral surfactant and an anionic surfactant, and the mixing ratio of the two types of surfactants is not limited.

2. The environmentally friendly nano hydrophobic emulsion according to claim 1, characterized in that: The active substance is a hydrogen-containing siloxane polymer, and the molecular formula of the hydrogen-containing siloxane polymer is: (R)3SiO[RHSiO] n Si(R)3, R = alkyl with 1 to 5 carbon atoms.

3. The environmentally friendly nano hydrophobic emulsion according to claim 2, characterized in that: The hydrogen content of the active material is 0.1%-1.7%.

4. The environmentally friendly nano hydrophobic emulsion according to claim 2, characterized in that: The neutral surfactant is a fatty alcohol, ether or ester compound, or a mixture thereof, and the mixing ratio is not limited; The anionic surfactant is a fatty sulfate, a fatty sulfonate, a fatty acid salt, or a mixture thereof, and the mixing ratio is not limited.

5. The environmentally friendly nano hydrophobic emulsion according to claim 4, characterized in that: The fatty alcohols are: containing at least one or more alcoholic hydroxyl groups (-OH) and saturated or unsaturated alkanes containing 6-30 straight-chain or branched carbons, and may also contain 0-3 carboxyl (-COO-) derivatives; The ethers are: saturated or unsaturated alkanes containing at least one or more ether groups (COC) and at least two straight or branched carbons with 6-30 carbon atoms, or derivatives of polyethylene glycol, HO[CH2CH2O] n -H (n = 100-100000); The ester compound is: a saturated or unsaturated fatty acid derivative (-COOC-) containing 6-30 straight-chain or branched carbons, and may also contain 0-5 alcoholic hydroxyl groups; The fatty acid or its salt can be: a saturated or unsaturated fatty acid (-COOH) or a fatty acid salt (-COOM, M = Na, K, Ca, etc.) containing 6-30 straight-chain or branched carbon atoms, or a fatty acid sulfate (ROSO3 - ), or fatty sulfonates (RSO3 - ).

6. A method for preparing an environmentally friendly nano hydrophobic emulsion, characterized in that: Dissolve the emulsifier in 50-80°C hot water in proportion, and mechanically stir the mixture for 30 minutes until a uniform emulsion is formed; when the emulsion temperature drops to about room temperature 25°C, adjust the pH value to 7±1 with a small amount of 10% hydrochloric acid or 10% sodium hydroxide solution; then stir the emulsion with a high shear machine, and slowly add the active ingredient at the same time. After the addition, continue to stir the mixture at high speed for 30 minutes until a uniform milky white emulsion is formed.

7. An application method of an environmentally friendly nano hydrophobic emulsion, characterized in that: Nano hydrophobic emulsion is mixed with mud, sand, soil, and clay to build dirt roads or earth roadbeds or other earth facilities with internal and external hydrophobicity. It can also be mixed with clay, sand, soil, and mud to prepare hydrophobic materials with different needs. The dosage of the hydrophobic material in the application is: the active matter in the nano hydrophobic emulsion is 0.05% to 2% of the weight of the clay, sand, soil, and earth material.

8. An application method of an environmentally friendly nano hydrophobic emulsion, characterized in that: A construction method for constructing a hydrophobic cement-soil highway or a hydrophobic cement-soil roadbed using hydrophobic materials; Surface hydrophobicity: Nano hydrophobic emulsion can be directly applied to the solid surface of inorganic materials. Its construction methods include painting, spraying, soaking, or wetting; Internal and external hydrophobicity: Nano hydrophobic emulsion can be directly mixed with soil, sand, and clay in a certain proportion and applied to build internal and external hydrophobic dirt roads, dirt roadbeds, dirt facilities, clay modification or controllable hydrophobicity, hydrophobic coatings, etc.

9. An application method of an environmentally friendly nano hydrophobic emulsion, characterized in that: Methods of constructing a sewerage soil road or roadbed: (1) Use road construction machinery to loosen the top 5-50 cm thick soil of the dirt road; (2) spraying a nano hydrophobic emulsion on loose dry soil, wherein the active substance in the nano hydrophobic emulsion is 0.001% to 5% of the weight of the dry soil; (3) Use road construction machinery such as a grader or tiller to evenly mix the soil and the hydrophobic material, and mix 90% of the soil into particles with a diameter of about 1 mm to 5 cm; (4) Use a grader or other machinery to make the mixed soil into an arched road surface according to the road construction method, and drainage facilities such as drainage ditches should be installed on both sides of the road; (5) A road roller or compactor is used to repeatedly press the road surface until a hard and smooth road surface is formed; (6) The wet dirt road needs a 2-10 day incubation and drying period until it forms a dry and hard porous dirt road. The incubation and drying time depends on the temperature and humidity of the environment. Generally, the ambient temperature should be above 20 degrees. Alternatively, the construction and application method of clay with controlled hydrophobic strength: The method of using nano-hydrophobic emulsion to treat soil, especially clay, with controllable hydrophobic strength is: (1) Use machinery such as an agricultural tiller to loosen the soil to a depth of 5-30 cm; (2) spraying the nano-hydrophobic emulsion evenly on the loose soil according to the experimental proportion, wherein the active substance in the nano-hydrophobic emulsion is 0.05% to 2% of the weight of the soil; (3) Use a tiller to evenly mix the soil and the sprayed nano-hydrophobic emulsion several times, and stir 90% of the soil into particles with a diameter of about 0.2 cm to 5 cm; dry it in a natural environment for 2-10 days, and then cultivate it after the treated soil is basically dry.

10. Use of the environmentally friendly nano hydrophobic emulsion according to any one of claims 1 to 5 in soil modification of muddy land that is not suitable for planting.