Preparation of hypercrosslinked macroporous adsorption resin for removing beta2-microglobulin in blood purification

By using the prepared ultra-high crosslinked macropore adsorption resin in blood purification, combined with the amination reaction to graft long-chain hydrophobic groups, the problem of low adsorption rate of β2-microglobulin in traditional hemodialysis methods is solved, and high efficiency is achieved blood purification effect.

CN118930958APending Publication Date: 2024-11-12SISHUI XIERKANG PHARMACELICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536447.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional hemodialysis methods are not effective in removing β2-microglobulin and parathyroid hormone from uremia patients, causing these toxins to accumulate in blood perfusion and affecting the patient's quality of life.

Method used

An ultra-high crosslinked macroporous adsorption resin prepared by suspension polymerization, chloromethylation and post-crosslinking reaction is used to graft long-chain hydrophobic groups in combination with the amination reaction to improve the adsorption performance of the resin.

Benefits of technology

It significantly improves the adsorption performance of β2-microglobulin, which is much higher than that of commercially available adsorbed materials, and reduces the adsorption of total protein, significantly improving the blood purification effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of hypercrosslinked macroporous adsorption resin for removing beta2-microglobulin in blood purification. The preparation method comprises the following steps: firstly, preparing macroporous styrene-divinylbenzene resin with a low crosslinking degree from styrene and divinylbenzene, and then carrying out secondary crosslinking on the macroporous styrene-divinylbenzene resin with the low crosslinking degree through a Friedel-Grafts method to prepare the hypercrosslinked adsorption resin. Residual chloromethyl is grafted with a long-chain hydrophobic group, so that the adsorption performance of the residual chloromethyl on beta2-microglobulin is further improved. The hypercrosslinked adsorption resin prepared by using the method has a huge specific surface area, abundant pore channels and very strong hydrophobic property, and has super-strong adsorption performance on beta2-microglobulin in the body of a uremia patient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of biomedical engineering, and in particular to a method for preparing an ultra-high cross-linked adsorption resin for removing beta 2-microglobulin in blood purification. Background Art

[0002] Hemoperfusion technology is a treatment method in which blood is introduced into a container filled with solid adsorbents with the help of an extracorporeal circulation power device to absorb and remove exogenous or endogenous toxins and metabolic products in the blood, and then return the purified blood to the body.

[0003] Uremic patients accumulate parathyroid hormone and β2-microglobulin in their blood at concentrations far higher than normal. With the increase in the number of traditional hemodialysis, parathyroid hormone and β2-microglobulin in the patient's body will accumulate and cannot be completely removed, causing a series of complications and seriously affecting the patient's quality of life. Hemoperfusion can effectively remove the residual high concentration of parathyroid hormone and β2-microglobulin in the body of uremic patients through the action of adsorbents, which is an effective supplement to hemodialysis.

[0004] At present, the adsorbents for hemoperfusion on the market have a low adsorption rate for β2-microglobulin in the blood. With the increasingly widespread application of hemoperfusion in the field of uremia, it is urgent to develop an adsorbent with strong adsorption performance for β2-microglobulin in the blood. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing an ultra-high cross-linked macroporous adsorption resin for removing β2-microglobulin in blood purification. The technical solution is as follows: The preparation of ultra-high cross-linked macroporous adsorption resin for removing β2-microglobulin in blood purification is characterized by comprising the following steps: Step 1: Preparation of macroporous styrene-divinylbenzene resin with low crosslinking degree A macroporous styrene-divinylbenzene resin with a low cross-linking degree is obtained by suspension polymerization using styrene monomers and polyvinyl cross-linking agents. The particle size of the resin ranges from 0.3 to 1.5 mm.

[0006] Step 2: Chloromethylation Take the macroporous styrene-divinylbenzene resin with low crosslinking degree prepared in step 1, add chloromethyl ether equivalent to 2-8 times the mass of the resin, let it stand at 30°C for 3-6 hours, add a catalyst equivalent to 0.2-2.0 times the mass of the resin under mechanical stirring, and react at 30-50°C for 5-80 hours to prepare chlorine balls.

[0007] Step 3: Post-crosslinking reaction Take the chlorine ball obtained in step 2, add a solvent equivalent to 3-8 times the mass of the chlorine ball, let it stand at 30-50°C for swelling for 3-6 hours, add a catalyst equivalent to 0.1-1.0 times the mass of the chlorine ball under mechanical stirring, heat and react at 75-130°C for 6-20 hours to prepare an ultra-high cross-linked macroporous adsorption resin.

[0008] Step 4: Grafting long-chain hydrophobic groups Take the ultra-high cross-linked macroporous adsorption resin in step 3, clean it with alcohol, and dry it. Add the swelling agent to the resin according to the mass ratio of resin: swelling agent = 1:2-8, swell for 2-4 hours, then add 10-20% of the resin mass of alkylamine, and heat to 70-100°C for 8-20 hours. During the reaction, gradually add NaOH solution to keep the pH value of the reaction system above 12, and the reaction obtains a finished product grafted with a long-chain hydrophobic group, which is washed with ethanol and water and dried.

[0009] Beneficial effects of the present invention: The preparation method of the ultra-high cross-linked macroporous adsorption resin for removing β2-microglobulin in blood purification of the present invention is adopted, styrene monomers and polyvinyl cross-linking agents are used to obtain macroporous styrene-divinylbenzene resin with low cross-linking degree through suspension polymerization, and then ultra-high cross-linked macroporous adsorption resin is prepared through chlorination and Friedel post-cross-linking, and finally long-chain alkyl is grafted onto the residual chloromethyl group through an amination reaction to prepare an ultra-high cross-linked macroporous adsorption resin with long-chain alkyl. It has a smooth surface and high strength, and has ultra-high adsorption performance for β2-microglobulin in uremic patients. DETAILED DESCRIPTION

[0010] The present invention is further described in detail below in conjunction with specific embodiments.

[0011] Embodiment 1: Suspension polymerization: In a 1000mL three-necked flask, add 500mL of an aqueous solution containing 1.2wt% gelatin, add 6g of divinylbenzene, 94g of styrene, 100g of n-hexanol, and a mixed oil phase of 1.0g of benzoyl peroxide. Under mechanical stirring, heat to 78°C and react for 4h, then heat to 83°C and solidify for 5h, then heat to 87°C and react for 6h. After the reaction, evaporate the porogen, wash with water until the washing liquid is clear, filter, dry, and sieve to select a resin with a particle size of 0.5-1.2mm to obtain a macroporous styrene-divinylbenzene resin with a low degree of crosslinking.

[0012] Chloromethylation Add 20g of the low cross-linking macroporous styrene-divinylbenzene resin obtained above into a 500mL three-necked flask, add 100g of chloromethyl ether, let stand at 30℃ for 4h, start the stirrer, add 20g of anhydrous zinc chloride twice, raise the temperature to 45℃ and react for 60h. After the reaction is completed, cool to room temperature, filter out the mother liquor, wash with methanol 3 times, wash with water until there is no methanol smell, filter with suction, and dry until the weight loss rate is less than 3% to obtain light yellow chlorine balls.

[0013] Post-crosslinking reaction Add 20 g of the above-obtained chlorine balls into a 500 mL three-necked flask, add 140 g of dichloroethane, let stand at 40 ° C for 4 h to swell, start mechanical stirring, add 5 g of ferric chloride, raise the temperature to 82 ° C, keep the reaction for 12 h, cool to room temperature, filter out the mother liquor, wash with alcohol three times and then with water until there is no alcohol smell, filter, and dry to obtain the ultra-high cross-linked macroporous adsorption resin.

[0014] Amination reaction According to the mass ratio of 1:2, dichloroethane was added to the ultra-high cross-linked macroporous adsorption resin to swell it, and it was swelled for 2 hours at room temperature. Then, 15% of the mass of n-hexylamine of the ultra-high cross-linked macroporous adsorption resin was added, and the temperature was raised to 80°C for reaction for 12 hours. During the reaction, a 20wt% NaOH solution of 3 times the mass of the alkylamine was gradually added dropwise to keep the pH value of the reaction system above 12. The ultra-high cross-linked macroporous adsorption resin grafted with long-chain hydrophobic groups was obtained by reaction. The resin was washed with alcohol 5 times and then washed with water until there was no alcohol smell, filtered, and dried.

[0015] Comparative Example 1: The ultra-high cross-linked macroporous adsorption resin obtained in step (3) of Example 1 is taken as Control Example 1.

[0016] Embodiment 2: (1) Suspension polymerization In a 1000mL three-necked flask, add 500mL of an aqueous solution containing 1.2wt% gelatin, add 6g of divinylbenzene, 94g of styrene, 100g of 200# gasoline, and a mixed oil phase of 1.0g of benzoyl peroxide. Under mechanical stirring, heat to 78℃ and react for 4h, then heat to 83℃ and solidify for 5h, then heat to 87℃ and react for 6h. After the reaction, evaporate the porogen, wash with water until the washing liquid is clear, filter, dry, sieve, and select a resin with a particle size of 0.5-1.2mm to obtain a macroporous styrene-divinylbenzene resin with a low degree of crosslinking.

[0017] (2) Chloromethylation reaction Add 20g of the low cross-linking macroporous styrene-divinylbenzene resin obtained above into a 500mL three-necked flask, add 100g of chloromethyl ether, let stand at 30℃ for 4h, start the stirrer, add 20g of anhydrous zinc chloride twice, raise the temperature to 45℃ and react for 60h. After the reaction is completed, cool to room temperature, filter out the mother liquor, wash with methanol 3 times, wash with water until there is no methanol smell, filter with suction, and dry until the weight loss rate is less than 3% to obtain light yellow chlorine balls.

[0018] (3) Post-crosslinking reaction Add 20 g of the above-obtained chlorine balls into a 500 mL three-necked flask, add 140 g of a mixed solvent of nitrobenzene and ethylene dichloride (nitrobenzene: ethylene dichloride = 1:1), let stand at 40°C for 4 h to swell, start mechanical stirring, add 5 g of ferric chloride, raise the temperature to 82°C, keep the temperature for reaction for 12 h, cool to room temperature, filter out the mother liquor, wash with alcohol three times and then with water until there is no alcohol smell, filter, and dry to obtain an ultra-high cross-linked macroporous adsorption resin.

[0019] (4) Amination reaction According to the mass ratio of 1:2, dichloroethane was added to the ultra-high cross-linked macroporous adsorption resin to swell it, and it was swelled for 2 hours at room temperature. Then, 15% of the mass of n-decylamine of the ultra-high cross-linked macroporous adsorption resin was added, and the temperature was raised to 80°C for reaction for 12 hours. During the reaction, a 20wt% NaOH solution of 3 times the mass of alkylamine was gradually added dropwise to keep the pH value of the reaction system above 12. The ultra-high cross-linked macroporous adsorption resin grafted with long-chain hydrophobic groups was obtained by reaction. The resin was washed with alcohol 5 times and then washed with water until there was no alcohol smell, filtered, and dried.

[0020] Comparative Example 2: The ultra-high cross-linked macroporous adsorption resin obtained in step (3) of Example 2 is taken as Control Example 2.

[0021] Embodiment 3: (1) Suspension polymerization In a 1000mL three-necked flask, add 500mL of an aqueous solution containing 1.2wt% gelatin, add 6g of divinylbenzene, 94g of styrene, 100g of ethyl acetate, and a mixed oil phase of 1.0g of benzoyl peroxide. Under mechanical stirring, heat to 78°C for reaction for 4h, then heat to 83°C for curing for 5h, and then heat to 87°C for reaction for 6h. After the reaction, evaporate the porogen, wash with water until the washing liquid is clear, filter, dry, and sieve to select a resin with a particle size of 0.5-1.2mm to obtain a macroporous styrene-divinylbenzene resin with a low degree of crosslinking.

[0022] (2) Chloromethylation reaction Add 20g of the low cross-linking macroporous styrene-divinylbenzene resin obtained above into a 500mL three-necked flask, add 100g of chloromethyl ether, let stand at 30℃ for 4h, start the stirrer, add 20g of anhydrous zinc chloride twice, raise the temperature to 45℃ and react for 60h. After the reaction is completed, cool to room temperature, filter out the mother liquor, wash with methanol 3 times, wash with water until there is no methanol smell, filter with suction, and dry until the weight loss rate is less than 3% to obtain light yellow chlorine balls.

[0023] (3) Post-crosslinking reaction Add 20 g of the above-obtained chlorine balls into a 500 mL three-necked flask, add 140 g of nitrobenzene, let stand at 40 ° C for 4 h to swell, start mechanical stirring, add 5 g of ferric chloride, raise the temperature to 120 ° C, keep the reaction for 12 h, cool to room temperature, filter out the mother liquor, wash with alcohol three times and then with water until there is no alcohol smell, filter, and dry to obtain the ultra-high cross-linked macroporous adsorption resin.

[0024] (4) Amination reaction According to the mass ratio of 1:2, dichloroethane was added to the ultra-high cross-linked macroporous adsorption resin to swell it, and it was swelled for 2 hours at room temperature. Then, 15% of the mass of n-hexadecylamine of the ultra-high cross-linked macroporous adsorption resin was added, and the temperature was raised to 80°C for reaction for 12 hours. During the reaction, a 20wt% NaOH solution of 3 times the mass of the alkylamine was gradually added dropwise to keep the pH value of the reaction system above 12. The ultra-high cross-linked macroporous adsorption resin grafted with long-chain hydrophobic groups was obtained by reaction. The resin was washed with alcohol 5 times and then washed with water until there was no alcohol smell, filtered, and dried.

[0025] Comparative Example 3: The ultra-high cross-linked macroporous adsorption resin obtained in step (3) of Example 3 is taken as Control Example 3.

[0026] Adsorption performance evaluation The plasma of patients with uremia (β2-MG concentration is 20 mg / L) was used to perform in vitro plasma adsorption experiments on the above examples and control examples. The experimental conditions were that the volume ratio of resin to plasma was 1 mL:20 mL, and the adsorption was carried out at 37°C and 60-80 rpm in a shaker for 2 hours. The results are shown in Table 1.

[0027] Table 1. Adsorption performance of the examples and reference examples on β2-MG and total protein serial number Adsorption rate (β2-MG) Adsorption rate (total protein) Example 1 95.7% 3.8% Comparative Example 1 90.7% 4.9% Example 2 94.2% 3.8% Comparative Example 2 89.6% 4.7% Example 3 98.8% 3.4% Comparative Example 3 91.3% 4.3% Commercially available adsorbent materials 78.2% 5.7%

[0028] It can be seen from Table 1 that: (1) The ultra-high cross-linked macroporous adsorption resin and the ultra-high cross-linked macroporous adsorption resin grafted with long-chain hydrophobic groups have super strong adsorption performance for β2-MG, which is much higher than that of commercially available adsorption materials, and their adsorption for total protein is lower than that of commercially available adsorption materials; (2) Grafting long-chain hydrophobic groups can significantly improve the adsorption of ultra-high cross-linked macroporous adsorption resin for β2-MG and reduce its adsorption for total protein.

[0029] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. For β 2 -Ultra-high cross-linked macroporous adsorption resin for microglobulin adsorption, Features: The following steps are involved: Step 1: Preparation of macroporous styrene-divinylbenzene resin with low crosslinking degree A macroporous styrene-divinylbenzene resin with a low degree of crosslinking is obtained by suspension polymerization using a styrene monomer and a polyvinyl crosslinking agent, wherein the particle size of the resin ranges from 0.3 to 1.5 mm; wherein the dispersion medium is water or saline, and the volume ratio of the dispersion medium to the oil phase is 2-4:1; the dispersant is any one of gelatin, polyvinyl alcohol, and cellulose or a mixture of several thereof, and the amount used is 0.2%-2.0% of the mass of the dispersion medium; the initiator is any one of benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate, and the amount used is 0.2%-2.0% of the total mass of the styrene monomer and the polyvinyl crosslinking agent; the porogen is any one of toluene, xylene, butanol, hexanol, cyclohexanol, n-heptane, 200# gasoline, liquid paraffin, solid paraffin, butyl acetate, ethyl acetate, and butyl butyrate, or a mixture of any two to three thereof, and the weight ratio of the porogen to the monomer is 60%-160%; Step 2: Chloromethylation Take the macroporous styrene-divinylbenzene resin with low crosslinking degree prepared in step 1, add chloromethyl ether equivalent to 2-8 times the mass of the resin, let it stand at 30° C. for 3- 6 hours, add a catalyst equivalent to 0.2-2.0 times the mass of the resin under mechanical stirring, and react at 30-50° C. for 5-80 hours to prepare chlorine balls, wherein the catalyst is one of zinc chloride, ferric chloride and aluminum chloride or a mixture of any two to three of them; Step 3: Post-crosslinking reaction Take the chlorine ball obtained in step 2, add a solvent equivalent to 3-8 times the mass of the chlorine ball, stand and swell at 30-50° C. for 3-6 hours, add a catalyst equivalent to 0.1-1.0 times the mass of the chlorine ball under mechanical stirring, and heat at 75-130° C. for 6-20 hours to prepare an ultra-high cross-linked macroporous adsorption resin, wherein the solvent is ethylene dichloride, nitrobenzene or a mixture of the two; the catalyst is one of zinc chloride, ferric chloride and aluminum chloride or a mixture of any two to three; Step 4: Grafting long-chain hydrophobic groups Take the ultra-high cross-linked macroporous adsorption resin in step 3, clean it with alcohol, dry it, add the swelling agent to the resin according to the mass ratio of resin: swelling agent = 1:2-8, swell for 2-4 hours, then add 10-20% of the mass of the resin alkylamine, and heat it to 70-100°C for 8-20 hours. During the reaction, NaOH solution is gradually added dropwise to keep the pH value of the reaction system above 12. The reaction obtains a finished product grafted with a long-chain hydrophobic group, and the finished product is washed with ethanol and water and dried, wherein the swelling agent is any one of dimethyl sulfoxide, dichloroethane or N, N-dimethylamide.

2. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The dispersion medium is water or salt water, and the volume ratio of the dispersion medium to the oil phase is 2-4:

1.

3. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The dispersant is any one of gelatin, polyvinyl alcohol and cellulose or a mixture of several thereof, and the dosage is 0.2%-2.0% of the mass of the dispersing medium.

4. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The initiator is any one of benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate, and the amount used is 0.2%-2.0% of the total mass of the styrene monomer and the polyvinyl crosslinking agent.

5. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The porogen is any one of toluene, xylene, butanol, hexanol, cyclohexanol, n-heptane, 200# gasoline, liquid paraffin, solid paraffin, butyl acetate, ethyl acetate, butyl butyrate, or a mixture of any two to three of them, and the weight ratio of the porogen to the monomer is 60%-160%.

6. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The catalyst used for chlorination and post-crosslinking is one of zinc chloride, ferric chloride and aluminum chloride or a mixture of any two to three thereof.

7. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The solvent used for post-crosslinking is ethylene dichloride, nitrobenzene or a mixture of the two.

8. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The post-crosslinking reaction steps are: adding a solvent equivalent to 3-8 times the mass of the chlorine ball, standing and swelling at 30-50°C for 3-6 hours, adding a catalyst equivalent to 0.1-1.0 times the mass of the chlorine ball under mechanical stirring, and heating and reacting at 75-130°C for 6-20 hours.

9. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The long-chain hydrophobic group is a C6-C18 alkyl group.

10. The method for removing β-catenin in blood purification according to claim 1. 2 -Preparation of ultra-high cross-linked adsorption resin for microglobulin, Features: The step of grafting long-chain hydrophobic groups onto an ultra-high cross-linked macroporous adsorption resin is as follows: taking an ultra-high cross-linked macroporous adsorption resin, cleaning it with alcohol, drying it, adding a swelling agent to the resin at a mass ratio of resin: swelling agent = 1:2-8, swelling for 2-4 hours, then adding alkylamine in an amount of 10-20% of the mass of the resin, and heating it to 70-100° C. to react for 8-20 hours, and gradually adding a NaOH solution dropwise during the reaction to keep the pH value of the reaction system above 12.