Light-color antistatic solid tire and preparation method thereof
By synergistically acting with the antistatic modifier and carbon nanotubes, a continuous conductive network is built, the contradiction between the conductivity and wear resistance of the antistatic tire is solved, and the efficient antistatic performance and stability of the tire is achieved, which is suitable for Various industrial environments.
Patent Information
- Application Number
- CN202411239200.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing antistatic solid tires are difficult to maintain wear resistance when improving conductivity, and the dark appearance limits the application range, and the performance stability in extreme environments is insufficient, affecting adaptability.
Using specific antistatic modifiers, a conductive path is formed through a π-electron system, and a continuous conductive network is constructed through vulcanization reaction. Combined with carbon nanotubes, the process flow is simplified, production costs are reduced, and the conductivity, wear resistance of the tire is ensured. stability.
It achieves excellent anti-static performance, good physical performance and light-colored appearance of the tire, improves the stability and adaptability of the tire, reduces production costs, and meets the industry's demand for efficiency and safety.
Smart Images

Figure BDA0005028701330000031 
Figure BDA0005028701330000061 
Figure BDA0005028701330000071
Abstract
Description
Technical Field
[0001] The invention relates to a light-colored antistatic solid tire and a preparation method thereof, belonging to the technical field of rubber. Background Art
[0002] In industrial automation and modern production systems, solid tires, as key components, play a vital role, especially in electrostatically sensitive industries such as electronics, medicine, and food. Although static electricity may seem insignificant, it can cause production safety problems, affect product quality, and even become a safety hazard under certain circumstances. Therefore, the research and development and application of anti-static solid tires can not only effectively prevent static electricity accumulation and ensure production safety, but also improve product quality and meet the industry's demand for an efficient and safe production environment. Especially in scenes such as dust-free workshops, precision instrument transportation, and electronic assembly lines, the importance of anti-static solid tires is self-evident. It can ensure the smooth operation of equipment, reduce failures and losses caused by static electricity, and provide solid technical support for modern production.
[0003] However, while achieving their electrostatic protection function, solid antistatic tires also face a series of technical challenges. First, in order to improve conductivity, traditional antistatic solid tires often add a large amount of conductive fillers, such as carbon black, metal fibers, etc., which can improve the antistatic performance of the tire, but at the same time lead to a significant decrease in the wear resistance of the tire, shorten the service life of the tire, and increase the maintenance cost of the enterprise. Secondly, the dark appearance of most antistatic tires limits their application in occasions with specific requirements for tire color, such as dust-free workshops. Light-colored tires are not only beautiful, but also easy to detect foreign objects. Furthermore, the performance stability of antistatic tires under extreme environmental conditions is insufficient. Changes in temperature and humidity will directly affect the antistatic effect of the tire, reducing its adaptability in different environments. These technical problems constitute the main bottleneck for improving the antistatic performance of solid tires.
[0004] In order to overcome the above technical obstacles, the industry and scientific researchers have actively explored and proposed a variety of technical means to improve antistatic performance. Among them, material modification is the most common method. Although the conductivity of the tire can be improved by adding specific conductive fillers to the rubber matrix, it is often difficult to resolve the contradiction between conductivity and wear resistance. Surface coating technology, that is, coating a conductive layer such as conductive carbon and metal oxides on the surface of the tire, can effectively reduce the surface resistance of the tire and maintain the original performance of the tire, but the cost is high and it is easy to wear during use, causing the antistatic effect to gradually decay over time. In recent years, the application of composite materials has become a research hotspot. By compounding new materials such as modified carbon nanotubes with rubber matrices, not only the conductivity of the tire is improved, but also the light color and high wear resistance of the tire can be maintained. However, the preparation process is complicated and the cost is high, which limits its large-scale application.
[0005] In summary, while improving the antistatic performance, solid antistatic tires need to solve problems such as wear resistance, color, and cost. The industry is actively exploring more comprehensive, economical, and efficient solutions to meet the growing industrial needs and promote the continuous innovation and progress of solid tire technology. Summary of the invention
[0006] In view of the defects of antistatic tires in the prior art, the first object of the present invention is to provide a light-colored antistatic solid tire. A specific antistatic modifier is introduced into the formula. The antistatic modifier has a large number of 3-hexylthiophene units, which can form a continuous conductive path through the π electron system, can effectively transmit and conduct the generated static charge, and through the vulcanization reaction, the base rubber forms a continuous conductive network, which significantly enhances the antistatic performance of the tire and can effectively reduce the use of conductive carbon, graphene and carbon nanotubes, so as to achieve the purpose of antistatic and light color.
[0007] The second object of the present invention is to provide a method for preparing a light-colored antistatic solid tire, which method uses a step-by-step mixing strategy to first ensure that the key antistatic components are evenly dispersed, and then add fillers for mixing, thereby simplifying the process flow, avoiding high-energy continuous mixing, and reducing production costs. At the same time, the rubber mixing technology of adding vulcanization accelerators step by step effectively controls the vulcanization process, ensures product quality, and the overall process is simple and efficient, which is conducive to large-scale production and has significant economic advantages.
[0008] In order to achieve the above technical objectives, the present invention provides a light-colored antistatic solid tire, which is made of the following raw materials in parts by weight: 40 to 75 parts of nitrile rubber, 1.5 to 4.0 parts of carbon nanotubes, 3 to 10 parts of antistatic modifier, 1.5 to 2.5 parts of antioxidant, 4.0 to 6.0 parts of resin, 4.5 to 5.5 parts of plasticizer, 4.0 to 5.0 parts of zinc oxide, 1.2 to 1.8 parts of vulcanization accelerator, 35 to 45 parts of white carbon black, 2.5 to 3.5 parts of silane coupling agent, 1.5 to 2.5 parts of polyethylene glycol, and 1.5 to 2.5 parts of stabilizer; the antistatic modifier is obtained by esterification reaction of poly (3-hexylthiophene-2,5-diyl) -hydroxy and carboxyl nitrile rubber.
[0009] The invention provides a light-colored antistatic solid tire, the innovation of which lies in the synergistic mechanism of the antistatic agent and the carbon nanotubes, which ensures that the tire has excellent electrical conductivity and antistatic performance, which is mainly reflected in the extended conjugated system constructed by the thiophene ring unit in the antistatic agent. The π electron system on each ring forms a chemical bond with the nitrile rubber through an esterification reaction. Combined with the vulcanization process, the conductive structure can be introduced into the three-dimensional structure after vulcanization, and a continuous and stable conductive network is constructed inside the tire. This network is interwoven with the highly conductive carbon nanotubes to jointly construct an efficient conductive path, so that static electricity can be quickly discharged and static electricity accumulation is effectively prevented. This mechanism not only significantly improves the antistatic effect of the tire, but also maintains the light-colored appearance of the tire. The chemical combination of the antistatic agent and the nitrile rubber , enhancing the physical properties of the tire, such as wear resistance and oil resistance, while the addition of carbon nanotubes further optimizes the structure of the conductive network and improves the stability and reliability of the antistatic performance. In addition, nitrile rubber as the main component in the formula gives the tire good elasticity and mechanical strength, carbon nanotubes and antistatic agents synergistically improve the conductivity of the tire, white carbon black and silane coupling agents enhance the physical properties and wear resistance of the tire, polyethylene glycol and stabilizers ensure the processing performance and stability of the tire, and the synergistic effect of each component is combined. The tire achieves excellent antistatic performance while maintaining good physical properties and light appearance, meets specific industrial and environmental needs, has significant technical and market advantages, and the overall formula and preparation method ensure the balance and excellence of the tire performance.
[0010] As a preferred solution, the antioxidant is at least one of 4010NA, RD and 6PPD; the resin is one of coumarone resin, terpene resin and rosin resin; the plasticizer is one of dioctyl phthalate, dioctyl terephthalate and polyisobutylene; the vulcanization accelerator is one of tetramethylthiuram disulfide, diphenylguanidine disulfide and N-cyclohexyl-2-benzothiazole sulfonamide; the stabilizer is one of zinc stearate, dibutyltin distearate and triphenylphosphine.
[0011] As a preferred solution, the chemical structure of the poly (3-hexylthiophene-2,5-diyl)-hydroxyl is as follows:
[0012]
[0013] The value of n is 30 to 150.
[0014] As a preferred solution, the conditions of the esterification reaction are: temperature of 45-80° C. and time of 6-18.
[0015] As a preferred solution, the mass ratio of the poly(3-hexylthiophene-2,5-diyl)-hydroxyl to the carboxylated nitrile rubber is 0.6 to 1.5: 1. By controlling the mass ratio, the amount of poly(3-hexylthiophene-2,5-diyl) in the tire is controlled, so that the mechanical properties and antistatic properties of the tire are balanced.
[0016] The present invention also provides a method for preparing a light-colored antistatic solid tire. The method comprises the following steps: mixing nitrile rubber, carbon nanotubes, an antistatic modifier, an antioxidant, a resin and a plasticizer according to weight proportions, performing a first kneading, then adding zinc oxide, white carbon black, a silane coupling agent, polyethylene glycol and a stabilizer for a second kneading to obtain a rubber compound, then adding a vulcanization accelerator for rubber refining to obtain a semi-finished tire embryo, and finally placing the semi-finished tire embryo in a mold for vulcanization treatment.
[0017] The preparation method of the present invention adopts step-by-step mixing, wherein nitrile rubber, antistatic agent and carbon nanotubes are mixed in advance to construct a preliminary conductive network, and the mixture can be evenly dispersed at the same time, and then white carbon black and the like are added to enhance the mechanical properties. Finally, a vulcanization accelerator is added to ensure efficient vulcanization, thereby achieving a balance between light color of the tire, excellent antistatic and physical properties, optimizing the processing flow, reducing energy consumption, improving production efficiency, combining innovative materials with processes, and meeting high industrial and environmental standards.
[0018] As a preferred solution, the conditions for the first mixing are: temperature of 100-125° C. and time of 20-35 min.
[0019] As a preferred solution, the second mixing conditions are: temperature of 80-100° C. and time of 10-25 min.
[0020] As a preferred solution, the temperature of the rubber mixing is 60-95°C.
[0021] As a preferred solution, the conditions of the vulcanization treatment are: temperature of 135-155°C, pressure of 9-11 kg / cm 2 , time is 40 to 65 minutes.
[0022] Compared with the prior art, the technical solution of the present invention brings about the following innovative and beneficial technical effects:
[0023] 1) The present invention introduces a conductive polymer with conjugated π bonds into nitrile rubber through careful design and compounding it with carbon nanotubes, and then performs a vulcanization reaction to construct a continuous and stable conductive network. The obtained antistatic tire has low resistance and can effectively conduct static charge, thereby ensuring the charge balance of the tire in various environments and improving safety performance.
[0024] 2) The present invention ensures the uniform dispersion of key ingredients such as carbon nanotubes and antistatic modifiers in the nitrile rubber matrix through a two-step mixing process. This not only enhances the mechanical strength and elasticity of the tire, but also further improves the durability and adaptability of the tire by precisely controlling the types and proportions of resins and plasticizers. At the same time, the vulcanization process is controlled so that the antistatic modifier and carbon nanotubes are effectively distributed in the three-dimensional network structure to achieve a balance between antistatic and mechanical properties.
[0025] 3) The light-colored antistatic solid tire provided by the present invention has excellent performance and high safety performance. The unique antistatic modifier significantly improves the charge dispersion efficiency and effectively prevents static electricity accumulation. The tire prepared by a reasonable formula shows high tensile strength, outstanding load-bearing capacity, and stable and reliable structure. The elongation at break is excellent, and it can be significantly stretched before deformation to fracture, which improves safety and durability. The Shao A hardness is moderate, ensuring wear resistance while having good ground adhesion and shock absorption effect. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be further described below in conjunction with specific embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; these embodiments are only for a better understanding of the present invention, rather than limiting the scope of protection of the present invention.
[0027] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0028] The poly(3-hexylthiophene-2,5-diyl)-hydroxyl used in the present invention was purchased from Angxing New Carbon Materials Changzhou Co., Ltd.
[0029] The commercially available powder antistatic agent used in the present invention is conductive titanium dioxide.
[0030] The commercially available liquid antistatic agent used in the present invention is polyquaternium-7.
[0031] Example 1
[0032] The preparation of the antistatic modifier is as follows:
[0033] First, 100g of poly(3-hexylthiophene-2,5-diyl)-hydroxyl with a number average molecular weight of 10000g / mol and 120g of carboxylated nitrile rubber were accurately weighed and dissolved in 2L of anhydrous DMF, heated to 60°C and stirred for 1h to ensure dissolution. Subsequently, 10g of dicyclohexylcarbodiimide and 4g of N,N'-dimethyl-4-dimethylaminopyridine were added in sequence, and stirring was continued at 60°C for 8h to promote the esterification reaction. After the reaction was completed, it was cooled to room temperature, and excess ethyl acetate was added to the mixture to precipitate the product. Unreacted raw materials and by-products were removed by filtration and washing. Finally, the precipitate was placed in a vacuum drying oven at 40°C and dried for 24h.
[0034] The preparation method of light-colored antistatic solid tire is as follows:
[0035] First, accurately weigh 70 parts of nitrile rubber, 2.5 parts of carbon nanotubes, 8 parts of antistatic modifier, 2 parts of 4010NA, 5 parts of coumarone resin, and 5 parts of dioctyl terephthalate, put them into an internal mixer, and mix them for the first time at 110°C for 30 minutes to obtain a preliminary mixed rubber. Cool the above rubber to room temperature, then add 4.5 parts of zinc oxide, 40 parts of white carbon black, 3 parts of silane coupling agent, 2 parts of polyethylene glycol, and 2 parts of dibutyltin distearate, and mix them for the second time at 85°C for 15 minutes to ensure uniform composition and obtain a rubber compound. The rubber compound is mixed at 65°C, and 1.5 parts of tetramethylthiuram disulfide are added and mixed until uniform to make a tire embryo. The tire embryo is placed in a mold and heated at 145°C and 8kg / cm 2 Vulcanize under pressure for 50 minutes to obtain a light-colored antistatic solid tire product.
[0036] Example 2
[0037] Compared with Example 1, the only difference is that 6PPD is used as the antioxidant and dioctyl phthalate is used as the plasticizer, and the other conditions and steps are the same.
[0038] Example 3
[0039] Compared with Example 1, the only difference is that the weight parts of the raw materials are different, and the other conditions and steps are the same. The weight parts of this embodiment are as follows: 70 parts of nitrile rubber, 2 parts of carbon nanotubes, 4 parts of antistatic modifier, 2 parts of 4010NA, 5 parts of coumarone resin, 5 parts of dioctyl terephthalate, 5 parts of zinc oxide, 44 parts of white carbon black, 3 parts of silane coupling agent, 2 parts of polyethylene glycol, 2 parts of dibutyltin distearate, and 1.5 parts of tetramethylthiuram disulfide.
[0040] Example 4
[0041] Compared with Example 1, the only difference is that the mass ratio of poly(3-hexylthiophene-2,5-diyl)-hydroxyl to carboxyl nitrile rubber is 1:1, and the other conditions and steps are the same.
[0042] Example 5
[0043] Compared with Example 1, the only difference is that the first mixing temperature is 120° C. and the time is 20 min, and the second mixing temperature is 95° C. and the time is 10 min. The other conditions and steps are the same.
[0044] Example 6
[0045] Compared with Example 1, the only difference is that the temperature of the esterification reaction is 55° C. and the time is 16 h, and the other conditions and steps are the same.
[0046] Comparative Example 1
[0047] Compared with Example 1, the only difference is that the antistatic modifier is replaced by a commercially available powder antistatic agent, and the other conditions and steps are the same.
[0048] Comparative Example 2
[0049] Compared with Example 1, the only difference is that the antistatic modifier is replaced by a commercially available liquid antistatic agent, and the other conditions and steps are the same.
[0050] Comparative Example 3
[0051] Compared with Example 1, the only difference is that no carbon nanotubes are added, and the other conditions and steps are the same.
[0052] Comparative Example 4
[0053] Compared with Example 1, the only difference is that the weight parts of the raw materials are different, and the other conditions and steps are the same. The weight parts of this comparative example are as follows: 65 parts of nitrile rubber, 5 parts of carbon nanotubes, 13 parts of antistatic modifier, 2 parts of 4010NA, 5 parts of coumarone resin, 5 parts of dioctyl terephthalate, 4.5 parts of zinc oxide, 37.5 parts of white carbon black, 3 parts of silane coupling agent, 2 parts of polyethylene glycol, 2 parts of dibutyltin distearate, and 1.5 parts of tetramethylthiuram disulfide.
[0054] Comparative Example 5
[0055] Compared with Example 1, the only difference is that the first mixing temperature is 95° C., the time is 15 min, the vulcanization temperature is 120° C., and the time is 70 min, and the other conditions and steps are the same.
[0056] The solid tires prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to performance tests, and the results obtained are shown in Table 1. The test standards are generally as follows:
[0057] Tensile strength: GB / T528-2009;
[0058] Elongation at break: GB / T 529-2008;
[0059] Abrasion resistance: GB / T 1689-2014;
[0060] Shore hardness: GGB / T 531.2-2009;
[0061] Resistance test: GB / T26277-2021.
[0062] Table 1 Performance test results of solid tires prepared in Examples 1 to 6 and Comparative Examples 1 to 5
[0063]
[0064]
[0065] In summary, the present invention significantly improves the comprehensive performance of solid tires through the optimized use of homemade antistatic modifiers, the appropriate addition of carbon nanotubes, and the precise control of mixing and vulcanization conditions. Compared with commercially available products, homemade antistatic modifiers not only improve the antistatic performance through synergy with base rubber, but also maintain the mechanical properties and wear resistance of the tire. The addition of carbon nanotubes further improves the antistatic performance, and effectively improves the tensile strength and elongation at break of the tire, showing its key performance enhancement effect. In addition, the mixing and vulcanization conditions in the preparation method of the present invention have a certain influence on the synergy of each formula of the raw materials, and then have an important influence on the tensile strength, Shore A hardness and other indicators of the tire.
[0066] The above embodiments are only for better explanation of the principles and practical applications of the present invention, so that those skilled in the relevant technical field can better understand and utilize the present invention, but they are not intended to limit the patent scope of the present invention. All equivalent changes made using the contents of the present invention are within the patent protection scope of the present invention.
Claims
1. A light-colored antistatic solid tire, characterized by: The invention is prepared from the following raw materials in parts by weight: 40-75 parts of nitrile rubber, 1.5-4.0 parts of carbon nanotubes, 3-10 parts of antistatic modifier, 1.5-2.5 parts of antioxidant, 4.0-6.0 parts of resin, 4.5-5.5 parts of plasticizer, 4.0-5.0 parts of zinc oxide, 1.2-1.8 parts of vulcanization accelerator, 35-45 parts of white carbon black, 2.5-3.5 parts of silane coupling agent, 1.5-2.5 parts of polyethylene glycol and 1.5-2.5 parts of stabilizer; the antistatic modifier is obtained by esterification reaction of poly(3-hexylthiophene-2,5-diyl)-hydroxyl and carboxyl nitrile rubber.
2. A light-colored antistatic solid tire according to claim 1, characterized in that: The antioxidant is at least one of 4010NA, RD and 6PPD; the resin is one of coumarone resin, terpene resin and rosin resin; the plasticizer is one of dioctyl phthalate, dioctyl terephthalate and polyisobutylene; the vulcanization accelerator is one of tetramethylthiuram disulfide, diphenylguanidine disulfide and N-cyclohexyl-2-benzothiazole sulfonamide; the stabilizer is one of zinc stearate, dibutyltin distearate and triphenylphosphine.
3. A light-colored antistatic solid tire according to claim 2, characterized in that: The chemical structure of the poly(3-hexylthiophene-2,5-diyl)-hydroxyl is as follows: The value of n is 30 to 150.
4. A light-colored antistatic solid tire according to claim 3, characterized in that: The conditions of the esterification reaction are: temperature of 45-80° C. and time of 6-18 hours.
5. A light-colored antistatic solid tire according to claim 4, characterized in that: The mass ratio of the poly(3-hexylthiophene-2,5-diyl)-hydroxyl group to the carboxyl nitrile rubber is 0.6-1.5:
1.
6. The method for preparing a light-colored antistatic solid tire according to any one of claims 1 to 5, characterized in that: The following steps are involved: According to the weight proportion, nitrile rubber, carbon nanotubes, antistatic modifier, antioxidant, resin and plasticizer are mixed for the first mixing, and then zinc oxide, white carbon black, silane coupling agent, polyethylene glycol and stabilizer are added for the second mixing to obtain a rubber compound, and then a vulcanization accelerator is added to mix the rubber to obtain a semi-finished tire embryo, and finally the semi-finished tire embryo is placed in a mold for vulcanization treatment.
7. The method for preparing a light-colored antistatic solid tire according to claim 6, characterized in that: The conditions for the first mixing are: temperature of 100-125° C. and time of 20-35 min.
8. The method for preparing a light-colored antistatic solid tire according to claim 6, characterized in that: The conditions for the second mixing are: temperature of 80-100° C. and time of 10-25 min.
9. The method for preparing a light-colored antistatic solid tire according to claim 6, characterized in that: The temperature of the rubber mixing is 60-95°C.
10. The method for preparing a light-colored antistatic solid tire according to claim 6, characterized in that: The conditions of the vulcanization treatment are: temperature of 135-155°C, pressure of 9-11 kg / cm 2 , time is 40 to 65 minutes.
Citation Information
Patent Citations
Conductive polymer composition, substrate and method for manufacturing substrate
CN115141448A
Conductive composition, conductive coating material, conductive resin, capacitor, photo-electric converting element, and process for producing the same
CN1806005A
Transparent conductive sheet for touch panel, manufacturing method thereof, and touch panel
JP2007095506A
Rubber composition for tire and tire manufactured by using the same
KR1020110073055A
Rubber composition for preventing electrostatic discharge of side wall
KR1020160043703A