Oil-resistant and wear-resistant rubber material for oil pressure equipment and preparation method of oil-resistant and wear-resistant rubber material

By uniformly mixing and curing the heat-resistant wear resin powder with Dingqing rubber latex, the problem of Dingqing rubber material wear in high temperature environments in large hydraulic equipment is solved, achieving higher wear and heat resistance, and extending The service life of the material.

CN118930998APending Publication Date: 2024-11-12DONGGUAN XINDONG RUBBER PLASTIC HARDWARE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411220926.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In high temperature and oil-containing environments, Dingqing rubber material is prone to wear, resulting in a reduced durability and is difficult to meet the needs of large-scale hydraulic equipment.

Method used

The heat-resistant wear emulsion obtained by emulsifying heat-resistant wear resin powder, silicone polyether copolymer, emulsifier and solvent in a specific proportion is fully mixed with the Dingqing rubber emulsion, and cured under the action of the crosslinking agent to form a high resistance. A rubber material that is thermal and wear-resistant.

Benefits of technology

It significantly reduces the wear phenomenon caused by friction in high temperature environments, improves the wear and heat resistance of rubber materials, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023006250000021
    Figure BDA0005023006250000021
  • Figure BDA0005023006250000031
    Figure BDA0005023006250000031
  • Figure BDA0005023006250000041
    Figure BDA0005023006250000041
Patent Text Reader

Abstract

The invention relates to the field of rubber materials, in particular to an oil-resistant and wear-resistant rubber material for oil pressure equipment and a preparation method of the oil-resistant and wear-resistant rubber material. The invention relates to an oil-resistant and wear-resistant rubber material for oil pressure equipment, which is characterized by being prepared from the following raw materials in percentage by weight: 64-80% of nitrile rubber buna emulsion, 5-10% of cross-linking agent, 9-30% of heat-resistant and wear-resistant emulsion and the balance of processing aid, the heat-resistant and wear-resistant emulsion is obtained by emulsifying heat-resistant and wear-resistant resin powder, an organosilicon polyether copolymer, an emulsifier and a solvent, the heat-resistant and wear-resistant emulsion and the nitrile rubber buna emulsion are fully mixed, so that the heat-resistant and wear-resistant resin powder is uniformly dispersed in the nitrile rubber buna emulsion, and under the action of the cross-linking agent, the heat-resistant and wear-resistant emulsion is obtained. The rubber material obtained after curing has better wear resistance and heat resistance. And when friction is carried out in a high-temperature and oil environment, the phenomenon of abrasion can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rubber materials, and more specifically, to an oil-resistant and wear-resistant rubber material for oil pressure equipment and a preparation method thereof. Background Art

[0002] Hydraulic equipment, also known as hydraulic press, is a machine that uses liquid pressure to process metal, plastic, rubber, wood, powder and other products. Its working principle is based on Pascal's law. It uses a hydraulic pump as a power source to convert mechanical energy into hydraulic energy, and then converts hydraulic energy into mechanical energy through a hydraulic cylinder to achieve pressure processing. Therefore, the materials used for hydraulic equipment usually have better oil resistance, pressure resistance, heat resistance and wear resistance.

[0003] Nitrile rubber has good resistance to wear and tear, so it is often used in the production of seals, hoses, hydraulic cylinders, pistons, hydraulic cylinders, buffers, shock absorbing parts, vulcanization tanks, etc. of hydraulic equipment, and can play a role in wear resistance and oil resistance.

[0004] However, the nitrile rubber used in large-scale hydraulic equipment tends to generate a lot of heat during operation, and heat is also generated when the nitrile rubber products are subjected to friction. Over time, it is easy to cause wear of the nitrile rubber products, thereby reducing the durability of the nitrile rubber. Summary of the invention

[0005] In order to reduce the wear and tear in a high temperature and oily environment, the present application provides a In a first aspect, an oil-resistant and wear-resistant rubber material for oil pressure equipment is characterized in that it is made of the following raw materials in percentage by weight: Nitrile rubber latex 64-80% Crosslinking agent 5-10% Heat-resistant wear emulsion 9-30% The balance is processing aids; The heat-resistant wear emulsion is obtained by emulsifying heat-resistant wear resin powder, silicone polyether copolymer, emulsifier and solvent in a weight ratio of (3-5): (0.1-0.5): (0.1-0.3): 10; The heat-resistant wear resin powder is prepared from one or more of organosilicon hybrid aromatic acetylene resin, polyetheretherketone and hydroxyl-terminated polyethersulfone.

[0006] The above technical scheme, through the heat-resistant wear resin powder, silicone polyether copolymer, emulsifier, solvent in a weight ratio of (3-5): (0.1-0.5): (0.1-0.3): 10 emulsification to obtain a heat-resistant wear emulsion, has better dispersibility and is easy to mix evenly with the nitrile rubber emulsion; and the heat-resistant wear resin powder prepared from one or more of silicone hybrid aromatic acetylene resin, polyether ether ketone, and hydroxyl-terminated polyether sulfone has high heat resistance, chemical corrosion resistance and wear resistance. Under the activation of the silicone polyether copolymer, the heat-resistant wear emulsion in an emulsified state is formed by the combination of the emulsifier and the solvent.

[0007] In summary, by fully mixing the heat-resistant wear emulsion with the nitrile rubber emulsion, the heat-resistant wear resin powder is evenly dispersed in the nitrile rubber emulsion, and under the action of the cross-linking agent, the rubber material obtained after curing has better wear resistance and heat resistance. When rubbed in a high temperature environment, the wear phenomenon can be reduced.

[0008] Preferably, the weight ratio of the organosilicon hybrid aromatic acetylene resin, polyetheretherketone, and hydroxyl-terminated polyethersulfone is 1:(3-5):(1-4).

[0009] The above-mentioned polyetheretherketone, organosilicon hybrid aromatic acetylene resin and hydroxyl-terminated polyethersulfone all have good heat resistance, and polyetheretherketone also has the advantages of good wear resistance and low friction. Therefore, when the three are compounded, their performance can be combined. For example, the hydroxyl group of hydroxyl-terminated polyethersulfone may form hydrogen bonds with the polar groups in PEEK or organosilicon hybrid aromatic acetylene resin, which helps to improve the interfacial bonding strength, and after blending, it has a synergistic effect to improve the thermal performance, and the heat-resistant wear resin powder obtained has better heat resistance and wear resistance, reduces the possibility of wear in high temperature environment, and improves its practicality.

[0010] When the organosilicon hybrid aromatic acetylene resin, polyetheretherketone and hydroxyl-terminated polyethersulfone are compounded, the heat-resistant wear-resistant resin powder is prepared by the following method: According to weight parts, polyetheretherketone and hydroxyl-terminated polyethersulfone are weighed and heated until completely melted, and the polyetheretherketone and hydroxyl-terminated polyethersulfone are fully mixed, cooled to 140°C, and organic silicon hybrid aromatic acetylene resin is added and mixed evenly, and then heated to 200°C to solidify the organic silicon hybrid aromatic acetylene resin, cooled to 30°C, and ground to obtain heat-resistant wear-resistant resin powder.

[0011] Preferably, the organosilicon hybrid arylacetylene resin is an organosilicon hybrid sulfur-containing arylacetylene resin and / or an organosilicon hybrid aromatic ether aromatic acetylene resin.

[0012] Organic silicon hybrid sulfur-containing aromatic acetylene resin is a silicon hybrid aromatic acetylene resin with a thioether structure in the main chain and an average molecular weight of 1000-2000; its molecular structure is as follows: The average molecular weight of organosilicon hybrid pyridine aryl acetylene resin is 1000-2000; its molecular structure is as follows: When the organosilicon hybrid sulfur-containing aromatic acetylene resin and / or the organosilicon hybrid aromatic ether aromatic acetylene resin are blended with polyetheretherketone and hydroxyl-terminated polyethersulfone, the obtained heat-resistant and wear-resistant resin powder has both good heat resistance and wear resistance, thereby further improving the heat resistance and wear resistance of the rubber material.

[0013] Preferably, the particle size of the heat-resistant wear-resistant resin powder is 0.01-5 microns.

[0014] The heat-resistant wear resin powder selected within the above particle size range has better dispersion effect and can provide better wear resistance. If the particle size of the heat-resistant wear resin powder is too small, its wear resistance effect is reduced, while if the particle size is too large, it will affect the physical properties of the rubber material.

[0015] Preferably, the nitrile rubber emulsion is one or more of carboxylated nitrile latex and / or hydrogenated nitrile latex.

[0016] Both carboxyl nitrile latex and hydrogenated nitrile latex have excellent oil resistance, chemical resistance and wear resistance, and are fully mixed with the heat-resistant wear emulsion. After curing, the formed rubber material has excellent wear resistance, heat resistance and oil resistance.

[0017] Hydrogenated nitrile latex is prepared from nitrile rubber latex by hydrogenation method, with a hydrogenation degree of 56-66% and a solid content of 50%.

[0018] Preferably, the weight ratio of the carboxylated nitrile latex, the hydroxylated nitrile latex and the hydrogenated nitrile latex is.

[0019] Preferably, the cross-linking agent is MOCA.

[0020] MOCA is 4,4'-methylenebis(2-chloroaniline) which plays a role in cross-linking and vulcanization, thereby further promoting the cross-linking and vulcanization of nitrile rubber emulsion and improving its comprehensive performance.

[0021] Preferably, the processing aid is one or more of a colorant, a filler, a release agent, and an antioxidant.

[0022] The above processing aids are used to play an auxiliary role, making the rubber material better able to meet the needs and improving its practicality.

[0023] In a second aspect, the present application provides a method for preparing an oil-resistant and wear-resistant rubber material for oil pressure equipment, comprising the following steps: According to the weight percentage, the nitrile rubber latex and the heat-resistant wear emulsion are weighed and mixed evenly to obtain a mixture A; the cross-linking agent is treated to obtain a treated cross-linking agent; the treated cross-linking agent and the mixture A are then mixed evenly to obtain a glue liquid, and the glue liquid is then transferred to a mold for mold molding to obtain an oil-resistant and wear-resistant rubber material.

[0024] The preparation method is simple to operate, and can make the heat-resistant wear emulsion fully and evenly dispersed in the nitrile rubber emulsion. After being evenly mixed with the cross-linking agent, the formed rubber liquid is molded into a mold, and the obtained oil-resistant wear-resistant rubber material has better wear resistance, heat resistance and oil resistance. After being applied to hydraulic equipment, the wear phenomenon during use is reduced, and its practicality is improved.

[0025] Preferably, the heat-resistant wear emulsion is prepared by the following method: The organosilicon polyether copolymer, emulsifier, solvent and heat-resistant wear resin powder are weighed, mixed evenly and emulsified to obtain a heat-resistant wear emulsion.

[0026] In the writing process, with the cooperation of silicone polyether copolymer, emulsifier and solvent, the heat-resistant and wear-resistant resin powder can be evenly dispersed and form a stable suspension after emulsification. At the same time, it is easy to be fully mixed with the nitrile rubber emulsion. Therefore, the obtained oil-resistant and wear-resistant rubber material has better wear resistance and heat resistance, reducing the phenomenon of friction and wear at high temperature.

[0027] In summary, this application has the following beneficial effects: 1. The heat-resistant wear emulsion is fully mixed with the nitrile rubber emulsion, so that the heat-resistant wear resin powder is evenly dispersed in the nitrile rubber emulsion. Under the action of the cross-linking agent, the rubber material obtained after curing has better wear resistance and heat resistance. When rubbed in a high temperature and oily environment, the wear phenomenon can be reduced.

[0028] 2. Polyetheretherketone, organosilicon hybrid aromatic acetylene resin and hydroxyl-terminated polyethersulfone all have good heat resistance, and polyetheretherketone also has the advantages of good wear resistance and low friction. Therefore, when the three are compounded, their performance can be combined. For example, the hydroxyl group of hydroxyl-terminated polyethersulfone may form hydrogen bonds with the polar groups in PEEK or organosilicon hybrid aromatic acetylene resin, which helps to improve the interfacial bonding strength, and after blending, it has a synergistic effect to improve the thermal performance. The heat-resistant and wear-resistant resin powder obtained thereby obtains better heat resistance and wear resistance, reduces the possibility of wear in high temperature environments, and improves its practicality. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] Introduction of some raw materials: Table 1 Introduction of some raw materials Example

[0031] Example 1 An oil-resistant and wear-resistant rubber material for oil pressure equipment is prepared by the following method: Heat-resistant wear resin powder, silicone polyether copolymer, emulsifier and solvent were weighed and mixed in a weight ratio of 3:0.1:0.3:10, and stirred at a speed of 100 r / min for 30 minutes to fully emulsify them to obtain a heat-resistant wear emulsion.

[0032] According to the weight percentage, the nitrile rubber latex and the heat-resistant wear emulsion are weighed and mixed, heated to 50°C, and stirred at 100 r / min for 5 hours to obtain a mixture A; the cross-linking agent is melted into a liquid state, the temperature is 80°C, and the time is 3 minutes to obtain a treated cross-linking agent; all the treated cross-linking agents are added to all the mixtures A and mixed evenly to obtain a glue solution; the glue solution is transferred to a mold, and molded at a temperature of 130°C and a time of 40 minutes to obtain an oil-resistant and wear-resistant rubber material.

[0033] The particle size of the heat-resistant wear resin powder is 5 microns; the heat-resistant wear resin powder is polyetheretherketone; the emulsifier is, the solvent is water; the nitrile rubber emulsion is carboxyl nitrile latex; the cross-linking agent is MOCA; and the processing aid is a colorant.

[0034] Example 2-3 The difference between Example 2-3 and Example 1 is that the amount of raw materials used is different, as shown in Table 2; Raw material weight percentage (%) of Examples 1-3 raw material Example 1 Example 2 Example 3 Nitrile rubber emulsion 64 70 80 Crosslinking agent 5 8 10 Heat and wear resistant emulsion 30 21 9 Color 1 1 1 Example 4 The difference between Example 4 and Example 2 is that the weight ratio of heat-resistant wear-resistant resin powder, silicone polyether copolymer, emulsifier and solvent is 4:0.3:0.2:10.

[0035] Example 5 The difference between Example 5 and Example 2 is that the weight ratio of heat-resistant wear-resistant resin powder, silicone polyether copolymer, emulsifier and solvent is 5:0.5:0.1:10.

[0036] Example 6 The difference between Example 6 and Example 4 is that the heat-resistant wear resin powder is obtained by the following method: Weigh polyetheretherketone and hydroxyl-terminated polyethersulfone, heat them until they are completely melted, mix them thoroughly and evenly, cool them to 140°C, add organosilicon hybrid aromatic acetylene resin and mix them evenly, heat them to 200°C again to solidify the organosilicon hybrid aromatic acetylene resin, cool them to 30°C, grind them, and obtain heat-resistant wear-resistant resin powder with a particle size of 5 microns.

[0037] The weight ratio of the organosilicon hybrid aromatic acetylene resin, polyetheretherketone and hydroxyl-terminated polyethersulfone is 1:3:1.

[0038] Example 7 The difference between Example 7 and Example 4 is that the weight ratio of the organosilicon hybrid aromatic acetylene resin, polyetheretherketone, and hydroxyl-terminated polyethersulfone is 1:5:2.

[0039] Example 8 The difference between Example 8 and Example 4 is that the weight ratio of the organosilicon hybrid aromatic acetylene resin, polyetheretherketone, and hydroxyl-terminated polyethersulfone is 1:5:4.

[0040] Example 9 The difference between Example 9 and Example 7 is that the particle size of the wear-resistant resin powder is 1 micron.

[0041] Example 10 The difference between Example 10 and Example 9 is that the organosilicon hybrid arylacetylene resin is composed of an organosilicon hybrid sulfur-containing arylacetylene resin and an organosilicon hybrid aryl ether arylacetylene resin in a weight ratio of 1:1.

[0042] Embodiment 11 The difference between Example 11 and Example 10 is that the nitrile rubber emulsion is composed of carboxyl nitrile latex and hydrogenated nitrile latex in a weight ratio of 3:1.

[0043] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the silicone polyether copolymer is replaced by heat-resistant resin powder in equal amount.

[0044] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that an equal amount of the heat-resistant resin powder is replaced with carbon black.

[0045] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the heat-resistant wear emulsion is replaced by an equal amount of nitrile rubber emulsion.

[0046] Performance testing Detection method / test method The oil-resistant and wear-resistant rubber materials obtained in Examples 1-11 and Comparative Examples 1-3 were cut into sizes for the following experiments and subjected to the following performance tests; Elongation and tensile strength: refer to ASTM D3574-17 for sampling and testing; Abrasion resistance: 1) Refer to "GB / T5478-2008 Plastic Rolling Wear Test Method", the sample diameter should be 100mm round sample 3pcs, thickness 0.8mm. Load 1kg; running length 25.4mm; speed 45 cycles / min; friction medium Cs-17; running times 3000 times; test environment temperature 85℃, humidity 60%. The proportion of wear of the test sample, take the average value, recorded as A,.

[0047] 2) The sample obtained in 1) is subjected to an aging treatment and then subjected to a wear resistance test under the same test conditions as 1); after the aging treatment condition is soaked in hydraulic oil at 120°C for 7 days, the wear amount ratio is tested and the average value is taken, recorded as B, and the wear increment = BA; Table 3 Examples 1-11 and Comparative Examples 1-3 Combining Example 1 and Comparative Examples 1-3 and Table 3, it can be seen that the elongation and tensile strength of Comparative Examples 1-3 are higher than those of Example 1, while the wear ratio and wear increment of Comparative Examples 1-3 are larger than those of Example 1, indicating that the heat-resistant wear emulsion obtained by emulsification of heat-resistant wear resin powder, silicone polyether copolymer, emulsifier and solvent has better wear resistance, physical properties and heat-resistant wear performance, and also has heat resistance and oil-resistant aging effects, so that the obtained rubber material can be used in large-scale hot pressing equipment to achieve better compression resistance, heat resistance, etc., and improve its durability.

[0048] By comparing Examples 6-8 with Example 4 and combining with Table 2, it can be seen that the wear amount of Example 4 accounts for nearly 2.1% or more, while the wear amount of Examples 6-8 accounts for less than 1.2%. After aging treatment, the wear of Example 4 increases to about 2.3%, while that of Example 6-8 is only about 1.2; in addition, the elongation and tensile strength of Examples 6-8 are higher than those of Example 4; this shows that the use of polyetheretherketone, organosilicon hybrid aromatic acetylene resin, and hydroxyl-terminated polyethersulfone plays a synergistic role, and the heat-resistant wear-resistant material formed by heat-resistant wear resin powder, organosilicon polyether copolymer, emulsifier, etc. is used in rubber materials, which plays a better dispersion and compatibility role, and can further improve the wear resistance, heat wear resistance, physical properties and aging wear resistance of rubber materials; therefore, when it is used in hydraulic equipment, it improves heat wear resistance, reduces wear and damage of parts of hydraulic equipment, and improves durability.

[0049] By comparing Example 10 with Example 9 and combining with Table 2, it can be seen that the elongation and tensile strength of Example 9 are higher than those of Example 10, while the wear amount ratio and wear increment of Example 10 are greater than those of Example 9, indicating that the compounding of the organosilicon hybrid sulfur-containing aromatic acetylene resin and the organosilicon hybrid aromatic ether aromatic acetylene resin has a synergistic effect, thereby making the obtained rubber material have better heat resistance, wear resistance and aging resistance.

[0050] By comparing Example 11 with Example 10 and combining with Table 2, it can be seen that the elongation and tensile strength of Example 11 are higher than those of Example 10, while the wear rate ratio and wear increment of Example 11 are greater than those of Example 10, indicating that the use of carboxyl nitrile latex and hydrogenated nitrile latex has a better synergistic effect, thereby making the comprehensive performance of the rubber material better.

[0051] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An oil-resistant and wear-resistant rubber material for oil pressure equipment, It is characterized in that Made from the following raw materials in weight percentage: Nitrile rubber emulsion 64-80% Crosslinking agent 5-10% Heat-resistant wear emulsion 9-30% The balance is processing aids; The heat-resistant wear emulsion is obtained by emulsifying heat-resistant wear resin powder, silicone polyether copolymer, emulsifier and solvent in a weight ratio of (3-5): (0.1-0.5): (0.1-0.3): 10; The heat-resistant wear resin powder is prepared from one or more of organosilicon hybrid aromatic acetylene resin, polyetheretherketone and hydroxyl-terminated polyethersulfone.

2. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 1, Features: The weight ratio of the organosilicon hybrid aromatic acetylene resin, polyetheretherketone and hydroxyl-terminated polyethersulfone is 1:(3-5):(1-4).

3. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 2, Features: The organosilicon hybrid arylacetylene resin is an organosilicon hybrid sulfur-containing arylacetylene resin and / or an organosilicon hybrid aryl ether arylacetylene resin.

4. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 1, Features: The particle size of the heat-resistant wear-resistant resin powder is 0.01-5 microns.

5. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 1, Features: The nitrile rubber emulsion is composed of one or more of carboxylated nitrile latex and / or hydrogenated nitrile latex.

6. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 5, Features: The weight ratio of the carboxyl nitrile latex to the hydrogenated nitrile latex is (2-5):

1.

7. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 1, Features: The cross-linking agent is MOCA.

8. The oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 1, Features: The processing aid is one or more of a colorant, a filler, a release agent, and an antioxidant.

9. A method for preparing the oil-resistant and wear-resistant rubber material for oil pressure equipment according to any one of claims 1 to 8, It is characterized in that The following steps are involved: According to the weight percentage, the nitrile rubber latex and the heat-resistant wear emulsion are weighed and mixed evenly to obtain a mixture A; the cross-linking agent is treated to obtain a treated cross-linking agent; the treated cross-linking agent and the mixture A are then mixed evenly to obtain a glue liquid, and the glue liquid is then transferred to a mold for mold molding to obtain an oil-resistant and wear-resistant rubber material.

10. The method for preparing the oil-resistant and wear-resistant rubber material for oil pressure equipment according to claim 9, It is characterized in that The heat-resistant wear emulsion is prepared by the following method: The organosilicon polyether copolymer, emulsifier, solvent and heat-resistant wear resin powder are weighed, mixed evenly and emulsified to obtain a heat-resistant wear emulsion.

Citation Information

Patent Citations

  • Oil-proof abrasion-resistant nylon 66 short fiber modified reinforced butadiene-acrylonitrile rubber seal plate and preparation method thereof

    CN106243422A

  • Preparation method of oil-resistant and high-temperature-resistant transformer sealing element

    CN111117025A

  • Nitrile rubber sealing ring

    CN112321915A

  • The Composion of Oil Seal and Oil Seal thereof

    KR1020110021251A