Antistatic regenerated PP composite material and preparation method thereof
By using composite antistatic agents formed by quaternary ammonium salt-type hyperbranched polysiloxane and white carbon black in recycled PP materials, the problem of easy breakage and electrostatic accumulation during processing is solved, and the material is efficient The antistatic performance and toughness are improved, reducing the risk of spark discharge.
Patent Information
- Application Number
- CN202411267279.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Recycled PP materials are prone to break during processing and are prone to static electricity, resulting in spark discharge risk and affecting safety.
Quaternary ammonium salt-type hyperbranched polysiloxane and white carbon black are used as composite antistatic agents. Through specific chemical reactions and mixing processes, a composite antistatic agent with core-shell structure is formed, combined with regenerated PP, antioxidants and lubricants. The antistatic regenerated PP composite material was prepared by melt forming by a twin-screw extruder.
It significantly improves the toughness and antistatic properties of recycled PP materials, reduces the risk of spark discharge, and enhances the safety and processing performance of the materials.
Smart Images

Figure BDA0005037506340000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic preparation, and in particular relates to an antistatic recycled PP composite material and a preparation method thereof. Background Art
[0002] PP (polypropylene) is a thermoplastic synthetic resin with good heat resistance and excellent bending fatigue resistance. It is widely used in automobiles, home appliances, office supplies, electronic appliances and other fields. Recycled PP came into being for the recycling of these PP products. Compared with new PP materials, recycled PP materials have lower toughness due to aging, are easy to break during blow molding or injection molding, and have poor processing performance. Therefore, the toughness of recycled PP is modified. At the same time, PP has strong insulation properties, and it is very easy to generate a large amount of static electricity accumulation during production and application, and it is difficult to eliminate it. If this large amount of accumulated static electricity is released, it will cause spark discharge, which is prone to explosion accidents. Therefore, it is necessary to improve a toughness-enhanced, anti-static recycled PP composite material and its preparation method. Summary of the invention
[0003] In view of the above problems, the present invention provides an antistatic recycled PP composite material and a preparation method thereof.
[0004] One object of the present invention can be achieved by the following technical solutions:
[0005] An antistatic recycled PP composite material comprises the following raw materials in parts by weight: 65-85 parts of recycled PP particles, 10-30 parts of composite antistatic agent, 0.5-3.5 parts of antioxidant, and 0.2-1.3 parts of lubricant;
[0006] The composite antistatic agent is obtained by mixing quaternary ammonium salt type hyperbranched polysiloxane and white carbon black with an auxiliary agent at 70-100° C. for 3-12 hours;
[0007] The quaternary ammonium salt type hyperbranched polysiloxane is prepared by quaternization reaction of tertiary ammonium hyperbranched polyurethane and γ-chloropropyltrimethoxysilane in a first organic solvent;
[0008] The tertiary amino hyperbranched polyurethane is prepared by photo-click reaction of terminal di-base hyperbranched polyurethane and 3-(dimethylamino)-1-propanethiol under the protection of a second organic solvent, a photosensitizer and nitrogen;
[0009] The terminal double-base hyperbranched polyurethane is prepared by thermal polymerization of hyperbranched polyester, diisocyanate and acrylic acid in the presence of a third organic solvent and a catalyst.
[0010] Furthermore, the mass ratio of the quaternary ammonium salt hyperbranched polysiloxane, white carbon black and the auxiliary agent is 10:1-2.5:3-6, and the auxiliary agent is a mixture of ethanol and water in any ratio.
[0011] Furthermore, the particle size of the white carbon black is 200-400 nm. The white carbon black not only plays the role of the inorganic core of the composite antistatic agent, but also has a certain conductivity and antistatic effect.
[0012] Preferably, the composite antistatic agent is obtained by the following reaction:
[0013] Add white carbon black and additives into a mixer, heat to 70-100°C while stirring, and spray quaternary ammonium salt hyperbranched polysiloxane. Continue to keep warm and stir for 3-12 hours after spraying, stop stirring, and dry to obtain a composite antistatic agent.
[0014] In the preparation reaction of the composite antistatic agent, the highly active silanol bond formed by the siloxane in the quaternary ammonium salt hyperbranched polysiloxane under the action of the auxiliary agent is used to form a bond chain with the hydroxyl group on the surface of white carbon black, thereby forming a composite antistatic agent with white carbon black as the core and the quaternary ammonium salt hyperbranched polysiloxane as the shell. The antistatic effect of white carbon black and the antistatic effect of the quaternary ammonium salt hyperbranched polysiloxane are utilized to improve the high-efficiency antistatic effect of the obtained composite antistatic agent, while improving the problem of easy agglomeration of traditional ultrafine white carbon black.
[0015] The composite antistatic agent not only plays the role of an antistatic agent, but also plays a toughening role of the core-shell structure. Remarkably, the quaternary ammonium salt type hyperbranched polysiloxane in the composite antistatic agent is an elastomer of hyperbranched polyurethane, and the toughening effect is more excellent.
[0016] Furthermore, the mass ratio of the tertiary ammonium hyperbranched polyurethane to γ-chloropropyltrimethoxysilane is 10:3-5, and the first organic solvent is one of isopropanol, benzene and chloroform.
[0017] Furthermore, the temperature of the quaternization reaction is 70-80° C., and the reaction time is 2-6 hours.
[0018] Preferably, the reaction obtained by the quaternary ammonium salt type hyperbranched polysiloxane is as follows:
[0019] After the tertiary ammonium hyperbranched polyurethane, γ-chloropropyltrimethoxysilane and the first organic solvent are uniformly mixed, the mixture is heated to 70-80° C. under condensation reflux, stirred and reacted for 2-6 hours, and the first organic solvent is recovered by rotary evaporation to obtain a light yellow liquid, i.e., a quaternary ammonium salt type hyperbranched polysiloxane.
[0020] Furthermore, the mass ratio of the terminal double-base hyperbranched polyurethane, 3-(dimethylamino)-1-propanethiol, and photosensitizer is 10:2-3:1.3-1.6, the second organic solvent is one of tetrahydrofuran, ether, acetone, and benzene, and the photosensitizer is benzoin dimethyl ether.
[0021] Furthermore, the reaction temperature of the photoclick reaction is 20-30°C, and the reaction time is 24-48h.
[0022] Preferably, the reaction for obtaining the tertiary aminated hyperbranched polyurethane is as follows:
[0023] The end-diyl hyperbranched polyurethane, 3-(dimethylamino)-1-propanethiol and the second organic solvent are uniformly mixed, and a photosensitizer is added under light-shielding and stirring. After nitrogen is passed, the mixture is irradiated with ultraviolet light of a wavelength of 365 nm at 20-30° C. for 24-48 hours (the reaction mixture is placed in a water bath during the entire reaction process to avoid ultraviolet light irradiation causing the temperature to be too high), and the second organic solvent is recovered by rotary evaporation, and then dissolved in chloroform and precipitated in n-hexane twice. The mixture is frozen in an ice storage and the upper clear liquid is poured off. The lower product is vacuum dried at low temperature (20-30° C.) to obtain a light yellow liquid, i.e., tertiary ammonium hyperbranched polyurethane.
[0024] Furthermore, the mass ratio of the hyperbranched polyester, diisocyanate, 1,4-butanediol and acrylic acid is 65-85:35-50:10-15:20-25, the third organic solvent is one of acetone, dimethylacetamide and benzene, and the first catalyst is one or more of organic tin catalysts.
[0025] Furthermore, the reaction temperature of the thermal polymerization reaction is 50-95° C., and the reaction time is 9-24 hours.
[0026] Preferably, the terminal double-base hyperbranched polyurethane is obtained by the following reaction:
[0027] After the hyperbranched polyester, diisocyanate, the first catalyst, 1,4-butanediol and the third organic solvent are uniformly mixed, heated to 50-95°C under nitrogen protection, stirred and reacted for 6-16 hours, then acrylic acid is added, and the stirring and reaction is continued for 3-8 hours. The reaction is stopped, the third organic solvent is recovered by rotary evaporation, washed with water, and dried to obtain a terminal di-base hyperbranched polyurethane.
[0028] Furthermore, the hyperbranched polyester is obtained by self-hyperbranching reaction of dihydroxymethylbutyric acid in the presence of a fourth organic solvent and a second reaction catalyst, wherein the second reaction catalyst is an esterification reaction catalyst well known in the technical field, such as sulfuric acid with a mass fraction of 98%, and the fourth organic solvent is one of tetrahydrofuran, dimethylacetamide, and benzene.
[0029] Preferably, the hyperbranched polyester is obtained by the following reaction:
[0030] The dimethylolbutyric acid and concentrated sulfuric acid are uniformly mixed in dimethylacetamide, heated to 70-80°C with stirring, and reacted for 4-6 hours, and then heated to 95-105°C, and then the dimethylolbutyric acid and concentrated sulfuric acid are continuously added to the reaction system, and the reaction is stirred and kept warm for 4-6 hours, and the reaction is stopped, and the dimethylacetamide is recovered by rotary evaporation, cooled, washed with water, and dried to obtain a hyperbranched polyester.
[0031] Another object of the present invention can be achieved by the following technical solutions:
[0032] A method for preparing an antistatic recycled PP composite material, characterized by comprising:
[0033] Adding recycled PP particles, composite antistatic agent, antioxidant and lubricant into a twin-screw extruder, and performing melt extrusion and molding to obtain an antistatic recycled PP composite material.
[0034] Beneficial effects of the present invention:
[0035] The present invention provides an antistatic recycled PP composite material and a preparation method thereof. The present invention not only achieves the antistatic performance of the PP composite material, but also improves the toughness of the recycled PP material by adding a composite antistatic agent, thereby solving the problems in the background technology. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Hyperbranched polyester: 0.1 mol dimethylolbutyric acid and concentrated sulfuric acid (the added mass is 3% of the mass of 0.1 mol dimethylolbutyric acid) are mixed evenly in 80 mL dimethylacetamide, heated to 75°C with stirring, and reacted for 5 hours, then heated to 95°C, and then 0.05 mol dimethylolbutyric acid and concentrated sulfuric acid (the added mass is 3% of the mass of 0.05 mol dimethylolbutyric acid) are continuously added to the reaction system, and the reaction is stirred and kept warm for 5 hours, the reaction is stopped, the dimethylacetamide is recovered by rotary evaporation, the temperature is lowered, the product is washed with water, and the product is dried to obtain a hyperbranched polyester, wherein the number average molecular weight of the obtained hyperbranched polyester is 2000-2500.
[0039] In the embodiments of the present invention, the hyperbranched polyester reaction adopts solvent reaction, which is convenient for obtaining hyperbranched polyester with narrow number average molecular weight. Secondly, the step-by-step reaction is adopted to facilitate further branching of the tree structure of the hyperbranched polyester.
[0040] In other embodiments of the present invention for preparing hyperbranched polyesters, a one-step reaction can also be performed, using dimethylolbutyric acid (AB2, A is a carboxyl group, and B is an alcoholic hydroxyl group) for self-hyperbranching reaction. The number average molecular weight of the hyperbranched polyester prepared by the one-step reaction of the present invention is 1000-2000, wherein the one-step reaction is specifically performed as follows:
[0041] 0.15 mol dihydroxymethylbutyric acid and concentrated sulfuric acid were mixed evenly in 80 mL dimethylacetamide, heated to 80°C with stirring, and reacted for 10 hours. The reaction was stopped, dimethylacetamide was recovered by rotary evaporation, cooled, washed with water, and dried to obtain hyperbranched polyester.
[0042] Example 2
[0043] Terminal double-base hyperbranched polyurethane:
[0044] 65 g of the hyperbranched polyester prepared in Example 1, 35 g of diisocyanate, 8 g of dibutyltin dilaurate, 10 g of 1,4-butanediol and 200 mL of dimethylacetamide were mixed evenly, heated to 75° C. under nitrogen protection, and stirred for reaction for 12 h. 20 g of acrylic acid was added, and the reaction was continued for 3 h. The reaction was stopped, and the dimethylacetamide was recovered by rotary evaporation, washed with water, and dried to obtain a terminal double-base hyperbranched polyurethane.
[0045] Example 3
[0046] Terminal double-base hyperbranched polyurethane:
[0047] 80 g of the hyperbranched polyester prepared in Example 1, 40 g of diisocyanate, 10 g of dibutyltin dilaurate, 15 g of 1,4-butanediol and 200 mL of dimethylacetamide were mixed evenly, heated to 95° C. under nitrogen protection, and stirred for 6 h. 25 g of acrylic acid was added, and the reaction was continued for 8 h. The reaction was stopped, and the dimethylacetamide was recovered by rotary evaporation, washed with water, and dried to obtain a terminal double-base hyperbranched polyurethane.
[0048] Example 4
[0049] Tertiary ammonium hyperbranched polyurethane:
[0050] 10 g of the terminal double-base hyperbranched polyurethane prepared in Example 2, 2 g of 3-(dimethylamino)-1-propanethiol and 40 mL of tetrahydrofuran were mixed uniformly, 1.3 g of benzoin dimethyl ether was added under stirring in the dark, and after nitrogen was passed, the mixture was irradiated with ultraviolet light having a wavelength of 365 nm at 20° C. for 24 h (the reaction mixture was placed in a water bath during the entire reaction process to avoid ultraviolet light irradiation causing the temperature to be too high), the second organic solvent was recovered by rotary evaporation, and then the mixture was dissolved in chloroform and precipitated in n-hexane twice, and the mixture was frozen in an ice bank and the supernatant was dumped off. The lower layer of the product was vacuum dried at low temperature (20-30° C.) to obtain a light yellow liquid, i.e., tertiary ammonium hyperbranched polyurethane.
[0051] Example 5
[0052] Tertiary ammonium hyperbranched polyurethane:
[0053] 10 g of the terminal double-base hyperbranched polyurethane prepared in Example 3, 3 g of 3-(dimethylamino)-1-propanethiol and 40 mL of tetrahydrofuran were mixed uniformly, 1.6 g of benzoin dimethyl ether was added under stirring in the dark, and after nitrogen was passed, the mixture was irradiated with ultraviolet light having a wavelength of 365 nm at 30° C. for 48 h (the reaction mixture was placed in a water bath during the entire reaction process to avoid ultraviolet light irradiation causing the temperature to be too high), the second organic solvent was recovered by rotary evaporation, and then the mixture was dissolved in chloroform and precipitated in n-hexane twice, and the mixture was frozen in an ice bank and the supernatant was dumped off. The lower layer of the product was vacuum dried at low temperature (20-30° C.) to obtain a light yellow liquid, i.e., tertiary ammonium hyperbranched polyurethane.
[0054] Example 6
[0055] Quaternary ammonium salt type hyperbranched polysiloxane:
[0056] 10 g of the tertiary ammonium hyperbranched polyurethane prepared in Example 4, 3 g of γ-chloropropyltrimethoxysilane and 60 mL of isopropanol were mixed evenly, heated to 70° C. under condensation reflux, stirred and reacted for 6 h, and the isopropanol was recovered by rotary evaporation to obtain a light yellow liquid, i.e., a quaternary ammonium salt hyperbranched polysiloxane.
[0057] Example 7
[0058] Quaternary ammonium salt type hyperbranched polysiloxane:
[0059] 10 g of the tertiary ammonium hyperbranched polyurethane prepared in Example 4, 5 g of γ-chloropropyltrimethoxysilane and 60 mL of isopropanol were mixed evenly, heated to 80° C. under condensation reflux, stirred and reacted for 2 h, and the isopropanol was recovered by rotary evaporation to obtain a light yellow liquid, i.e., a quaternary ammonium salt type hyperbranched polysiloxane.
[0060] Example 8
[0061] Composite antistatic agent:
[0062] 10g of white carbon black and 30g of an auxiliary agent (ethanol: water mass ratio of 4:1) were added to a blender, heated to 80°C while stirring, and 100g of the quaternary ammonium salt hyperbranched polysiloxane prepared in Example 6 was sprayed. After spraying, the mixture was kept warm and stirred for 6h, stirring was stopped, and the mixture was dried to obtain a composite antistatic agent, wherein the particle size of the white carbon black was 200-300nm.
[0063] Example 9
[0064] Composite antistatic agent:
[0065] 25 g of white carbon black and 60 g of an auxiliary agent (ethanol: water mass ratio of 4:1) were added to a blender, heated to 90°C while stirring, and 100 g of the quaternary ammonium salt hyperbranched polysiloxane prepared in Example 7 was sprayed. After spraying, the mixture was kept warm and stirred for 12 h, stirring was stopped, and the mixture was dried to obtain a composite antistatic agent, wherein the particle size of the white carbon black was 200-300 nm.
[0066] Comparative Example 1
[0067] Control group 1: composite antistatic agent
[0068] Add 10g of white carbon black and 30g of an auxiliary agent (ethanol:water mass ratio is 4:1) into a blender, heat to 80°C while stirring, and spray 100g of γ-chloropropyltrimethoxysilane. Continue to keep warm and stir for 6 hours after spraying, stop stirring, and dry to obtain a composite antistatic agent, wherein the particle size of the white carbon black is 200-300nm.
[0069] Comparative Example 2
[0070] Control group 2: the antistatic agent is white carbon black with a particle size of 200-300 nm.
[0071] Example 10
[0072] Antistatic recycled PP composite material
[0073] Prepare the following raw materials in parts by weight: 65 parts of recycled PP particles, 30 parts of the composite antistatic agent prepared in Example 8, 0.5 parts of antioxidant, and 0.2 parts of lubricant; add the prepared recycled PP particles, composite antistatic agent, antioxidant and lubricant into a twin-screw extruder, and obtain an antistatic recycled PP composite material by melt extrusion and molding. The antioxidant is antioxidant 1010, and the lubricant is polypropylene.
[0074] Embodiment 11
[0075] Antistatic recycled PP composite material
[0076] Prepare the following raw materials in parts by weight: 70 parts of recycled PP particles, 20 parts of the composite antistatic agent prepared in Example 9, 1.5 parts of antioxidant, and 1 part of lubricant; add the prepared recycled PP particles, composite antistatic agent, antioxidant and lubricant into a twin-screw extruder, and obtain an antistatic recycled PP composite material by melt extrusion and molding. The antioxidant is antioxidant 1010, and the lubricant is polypropylene.
[0077] Example 12
[0078] Antistatic recycled PP composite material
[0079] Prepare the following raw materials in parts by weight: 85 parts of recycled PP particles, 10 parts of the composite antistatic agent prepared in Example 8, 3.5 parts of antioxidant, and 1.3 parts of lubricant; add the prepared recycled PP particles, composite antistatic agent, antioxidant and lubricant into a twin-screw extruder, and obtain an antistatic recycled PP composite material by melt extrusion and molding. The antioxidant is antioxidant 1010, and the lubricant is polypropylene.
[0080] Comparative Example 3
[0081] Antistatic recycled PP composite material: Compared with Example 10, an equal amount of the composite antistatic agent is replaced with the composite antistatic agent prepared in Comparative Example 1, and the rest is the same.
[0082] Comparative Example 4
[0083] Antistatic recycled PP composite material: Compared with Example 10, an equal amount of the composite antistatic agent is replaced with the antistatic agent in Comparative Example 2, and the rest is the same.
[0084] Comparative Example 5
[0085] Antistatic recycled PP composite material: Compared with Example 10, an equal amount of the composite antistatic agent is replaced with the quaternary ammonium salt type hyperbranched polysiloxane prepared in Example 6, and the rest is the same.
[0086] Comparative Example 6
[0087] Antistatic recycled PP composite material: Compared with Example 10, the composite antistatic agent is deleted, and the rest is the same.
[0088] The physical properties of the antistatic recycled PP composite material prepared above were tested, and the test results are shown in Table 1. Among them, the tensile properties were tested according to GB / T528; the tear strength: according to GB / T 529; the surface resistance: tested using a PC68 digital high resistance meter, the test conditions: the sample was dried before testing and placed in an oven at 80°C for 4 hours; the voltage in the test was selected as 1000 volts;
[0089] Table 1
[0090]
[0091] It can be seen from the data in Table 1 that the antistatic recycled PP composite materials obtained in Examples 10-11 of the present invention have good elastic properties and antistatic properties.
[0092] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0093] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An antistatic recycled PP composite material, characterized in that: The raw materials include the following parts by weight: 65-85 parts of recycled PP particles, 10-30 parts of composite antistatic agent, 0.5-3.5 parts of antioxidant, and 0.2-1.3 parts of lubricant; The composite antistatic agent is obtained by mixing quaternary ammonium salt type hyperbranched polysiloxane and white carbon black with an auxiliary agent at 70-100° C. for 3-12 hours; The quaternary ammonium salt type hyperbranched polysiloxane is prepared by quaternization reaction of tertiary ammonium hyperbranched polyurethane and γ-chloropropyltrimethoxysilane in a first organic solvent; The tertiary amino hyperbranched polyurethane is prepared by photo-click reaction of terminal di-base hyperbranched polyurethane and 3-(dimethylamino)-1-propanethiol under the protection of a second organic solvent, a photosensitizer and nitrogen; The terminal double-base hyperbranched polyurethane is prepared by thermal polymerization of hyperbranched polyester, diisocyanate, 1,4-butanediol and acrylic acid in the presence of a third organic solvent and a catalyst.
2. The antistatic recycled PP composite material according to claim 1, characterized in that: The mass ratio of the quaternary ammonium salt type hyperbranched polysiloxane, white carbon black and the auxiliary agent is 10:1-2.5:3-6, and the auxiliary agent is ethanol or water or a mixture of the two in any ratio.
3. The antistatic recycled PP composite material according to claim 1, characterized in that: The mass ratio of the tertiary ammonium hyperbranched polyurethane to γ-chloropropyltrimethoxysilane is 10:3-5, and the first organic solvent is one of isopropanol, benzene and chloroform.
4. The antistatic recycled PP composite material according to claim 1, characterized in that: The temperature of the quaternization reaction is 70-80° C., and the reaction time is 2-6 hours.
5. The antistatic recycled PP composite material according to claim 1, characterized in that: The mass ratio of the terminal double-base hyperbranched polyurethane, 3-(dimethylamino)-1-propanethiol and photosensitizer is 10:2-3:1.3-1.6, the second organic solvent is one of tetrahydrofuran, ether, acetone and benzene, and the photosensitizer is benzoin dimethyl ether.
6. The antistatic recycled PP composite material according to claim 1, characterized in that: The reaction temperature of the photoclick reaction is 20-30°C, and the reaction time is 24-48h.
7. The antistatic recycled PP composite material according to claim 1, characterized in that: The mass ratio of the hyperbranched polyester, diisocyanate, 1,4-butanediol and acrylic acid is 65-85:35-50:10-15:20-25, the third organic solvent is one of acetone, dimethylacetamide and benzene, and the first catalyst is one or more of organic tin catalysts.
8. The antistatic recycled PP composite material according to claim 1, characterized in that: The reaction temperature of the thermal polymerization reaction is 50-95° C., and the reaction time is 9-24 hours.
9. The antistatic recycled PP composite material according to claim 1, characterized in that: The hyperbranched polyester is obtained by self-hyperbranching reaction of dimethylolbutyric acid in the presence of a fourth organic solvent and a second catalyst.
10. The method for preparing an antistatic recycled PP composite material according to claims 1-9, characterized in that: include: Adding recycled PP particles, composite antistatic agent, antioxidant and lubricant into a twin-screw extruder, and performing melt extrusion and molding to obtain an antistatic recycled PP composite material.
Citation Information
Patent Citations
Lasting and effective antistatic polyolefin composite material and preparation method thereof
CN104448506A
Antistatic treating agent and preparation method thereof
CN107501520A
Preparation method of antistatic high-strength PP material
CN114456497A
Wear-resistant antistatic plastic, preparation method thereof and application of wear-resistant antistatic plastic in trundle preparation
CN118562221A
Modifiers for polyurethane resins
JP1977045654A