Preparation method of high-wear-resistance and high-temperature-resistance lining plate for preparation equipment

By pretreatment and segmented calcination of coal gangue powder, combined with the use of specific additives, high wear-resistant and high temperature-resistant gangue masterbatches are prepared and blended with ABS resin, which solves the wear resistance of the lining material in the prior art. As well as the problem of insufficient high temperature resistance, the cost-effective preparation of lining sheet materials for ore dressing equipment has been achieved, significantly improving the service life of the equipment and the comprehensive utilization value of the materials.

CN118931097APending Publication Date: 2024-11-12ZHENGZHOU MINERALS COMPOSITIVE UTILIZATION RES INST CHINESE GEOLOGICAL ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979952.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing ore dressing equipment lining materials have limitations in preparation methods, material composition or process, and it is difficult to achieve high wear resistance and high temperature resistance at the same time, and it is cost-effective and lacks cost-effective solutions.

Method used

The coal gangue powder with low quartz content was pretreated, calcined in sections and additives to prepare high wear and high temperature gangue masterbatch, and blended with ABS resin, and prepare the liner by extrusion blending process. Specific additives are added to improve the utilization efficiency and crystal structure of quartz and clay.

Benefits of technology

It significantly improves the wear resistance and high temperature resistance of the lining plate, reduces production costs, extends the service life of ore dressing equipment, and improves the comprehensive utilization value of coal gangue, realizing the preparation of high-value products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955748170000051
    Figure BDA0004955748170000051
Patent Text Reader

Abstract

The invention provides a preparation method of a high-wear-resistance and high-temperature-resistance lining plate for preparation equipment. The method comprises the following steps: firstly, pretreating coal gangue to obtain coal gangue powder with low quartz content; then, the powder is subjected to segmented calcination, and the whiteness and purity of the powder are improved by accurately controlling the calcination temperature and time. And finally, mixing the calcined powder with an additive solution in a preset proportion, and preparing the coal gangue functional filler master batch with high wear resistance and high temperature resistance through an extrusion blending technology. And blending the coal gangue master batch with ABS resin to prepare the high-wear-resistance and high-temperature-resistance lining plate. According to the invention, coal gangue resources can be efficiently utilized, the prepared master batch shows excellent wear resistance and high temperature resistance, and is suitable for industries such as rubber and plastic, the material performance is remarkably improved, the production cost is reduced, and good economic benefits and social benefits are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lining plates for ore dressing equipment, in particular to a method for preparing a lining plate for ore dressing equipment with high wear resistance and high temperature resistance. Background Art

[0002] At present, some researchers have made some progress in the research and development of lining materials for mineral processing equipment. For example, the invention patent application with application publication number CN110655699A discloses an energy-saving and wear-resistant mill rubber lining, which is vulcanized from an energy-saving and wear-resistant rubber composite material, and the rubber composite material is composed of the following components by weight: 250 parts of tin-coupled solution-polymerized styrene-butadiene rubber SSBR-SL55, 20-30 parts of natural rubber NR, 20-30 parts of butadiene rubber BR9000, 4-6 parts of zinc oxide, 1-3 parts of stearic acid, 1.5-2.0 parts of sulfur, 1.5-2.0 parts of accelerator, 2-3 parts of antioxidant, 1-2 parts of protective wax, and anti-scorch agent CTP 0.5-1 parts, low rolling resistance carbon black 25-30 parts, high dispersion white carbon black 25-30 parts, silane coupling agent (i692-4 parts, CMoSSi wear agent 4-6 parts, coumarone resin 5-7 parts, aromatic oil 3-5 parts. The invention patent application with application publication number CN104354239A discloses a method for preparing wear-resistant linings using ultra-high molecular weight polyethylene composite waste, which is to place ultra-high molecular weight polyethylene composite waste treated in a solvent in a specific mold, and press it into a wear-resistant lining on a flat vulcanizer under certain temperature and pressure conditions. Among them, the ultra-high molecular weight polyethylene fiber composite waste is the scraps generated when producing armor protection products.

[0003] However, these existing inventions have certain limitations in preparation methods, material composition or preparation process. Therefore, it is still of great practical significance to develop a lining material for mineral processing equipment that is simple to prepare, low in cost, and has high wear resistance and high temperature resistance. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a liner for a highly wear-resistant and high-temperature resistant ore dressing equipment, which specifically includes the following technical solutions:

[0005] Step 1: preparing coal gangue powder with low quartz content, wherein the quartz content of the coal gangue powder is 10%-20%; Step 1 specifically comprises:

[0006] Step 1.1: Pre-treating and crushing the coal gangue, wherein the particle size after crushing is D50≤20mm; the quartz content in the coal gangue is greater than 50%;

[0007] Step 1.2: Add 0.2-5% additive A to the crushed coal gangue, grind it with a jet mill, obtain product 1 at the discharge port, and obtain product 2 in the dust removal bag; the additive A is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1-2:1-2:0.5-3.

[0008] Step 1.3: Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0009] Step 1.4: Product 2 and Product 3 are mixed and then crushed again to obtain a powder with a D97 of 18 μm.

[0010] Step 2: calcining the gangue powder in stages; Step 2 specifically comprises:

[0011] Add 3-5% of additive B to the gangue powder obtained in step 1, perform segmented calcination, and finally crush to 800 mesh; the additive B is prepared by mixing sodium chloride, boric acid, and magnesium sulfate in a mass ratio of 3-5:1-2.5:0.5-2. The segmented calcination parameters are: the first segment is heated from room temperature to 350°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes; the second segment is heated to 750°C, the heating rate is 20°C / min, and the temperature is kept for 10 minutes; the third segment is heated to 850-900°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes, and quenched to 300°C, and then naturally cooled to room temperature.

[0012] Step 3: using the product obtained in step 2 to prepare a highly wear-resistant and high-temperature resistant coal gangue masterbatch; step 3 comprises:

[0013] Step 3.1: Add the additive C solution to the product obtained in step 2, stir and blend to obtain a filler; in the filler, the additive C solution accounts for 3-6wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan; in the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan is 3-4:1-2:1-2.

[0014] Step 3.2: Extrusion blend the filler obtained in step 3.1 according to 60% filler and 40% matrix resin to prepare coal gangue masterbatch. Specifically, the filler mixed in step 3.1 is first stirred at 105° C. for 1 hour, and then the mixed filler and matrix resin are extruded and blended. The matrix resin is PP-maleic anhydride or ABS.

[0015] Step 4: Blend the gangue masterbatch with the matrix resin to prepare a high wear-resistant and high-temperature resistant lining plate. The mass ratio of the gangue masterbatch to the ABS resin is 20-30%:70-80%.

[0016] According to the test, the liner prepared by the present invention has excellent wear resistance and high temperature resistance. Compared with the ABS liner without filler, the thermal deformation temperature of the liner with 20% masterbatch added can be increased to 120°C, and the mass wear can be reduced to 0.4g.

[0017] The beneficial effects of the present invention include:

[0018] The invention improves the comprehensive utilization value of coal gangue; the prepared masterbatch has high wear resistance and high temperature resistance; the process flow is simple and the production cost is low; through staged calcination and adding additives, the quartz and clay in the coal gangue are effectively utilized; the prepared masterbatch can be widely used in the field of rubber and plastic materials to improve the wear resistance and high temperature resistance of rubber and plastic materials.

[0019] (1) The present invention uses low-value coal gangue with a quartz content greater than 50% as raw material to prepare high-value, highly wear-resistant and high-temperature-resistant masterbatch, converting low-value minerals into high-value products, significantly improving economic efficiency.

[0020] (2) The present invention can effectively reduce the impurity content by adding additives of specific composition when crushing coal gangue, and can also better separate quartz and silicate clay, thereby improving the separation efficiency. In addition, the quartz content is ensured to be maintained at 10%-20% by combining the screening of particle sizes after multiple crushings. Because the appropriate amount of quartz changes its phase after subsequent calcination, the wear resistance of the product can be improved.

[0021] (3) The present invention adds additives in a specific proportion when calcining the gangue powder in stages, wherein the purpose of the staged calcination is, first, to remove impurities and improve whiteness; second, to help regulate the crystal form, change the quartz structure, and improve wear resistance. The first stage of calcination removes organic matter, the second stage of calcination removes iron, and the third stage of calcination causes the silicon-aluminum ratio to change in the physical phase structure under specific temperature, insulation time, and quenching conditions to form a special structure, which is beneficial for preparing powders and improving the wear resistance and high temperature resistance of later products. The addition of additives can synergistically improve its high temperature resistance and changes in the crystal structure, which is beneficial for phase reconstruction and improves overall wear resistance and high temperature resistance.

[0022] (4) The liner prepared by the present invention has excellent wear resistance and high temperature resistance, and can significantly improve the service life of the mineral processing equipment. Compared with the existing ABS liner, the liner prepared by the present invention has significant advantages in wear resistance and high temperature resistance. DETAILED DESCRIPTION

[0023] The present invention is described in more detail below through specific implementation modes to facilitate understanding of the technical solution of the present invention, but is not intended to limit the protection scope of the present invention.

[0024] Example 1

[0025] Raw materials: coal gangue from a certain region, quartz content is 55wt% and clay content is 30wt%.

[0026] Preparation process of lining plate for mineral processing equipment in this embodiment:

[0027] Step 1. Pre-treat and crush the gangue to a particle size of D50≤20mm after crushing;

[0028] Step 2. Put the crushed coal gangue into a fluidized bed jet mill, add 0.2wt% of additive A, and crush once by adjusting the classifying wheel, and obtain product 1 at the discharge port and product 2 in the dust removal bag; wherein the additive is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1:1:0.5;

[0029] Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0030] Step 4. Mix product 2 and product 3 and grind them twice to obtain a powder with a D97 of 18 μm, i.e., product 4;

[0031] Step 5. Add 3wt% of additive B to product 4, where additive B is mixed with sodium chloride, boric acid and magnesium sulfate in a mass ratio of 3:1:0.5; calcine in stages through a muffle furnace, a rotary kiln or a microwave calcining furnace, heating to 350°C in the first stage, heating rate of 10°C / min, and keeping warm for 30 minutes; heating to 750°C in the second stage, heating rate of 20°C / min, and keeping warm for 10 minutes; heating to 850°C in the third stage, heating rate of 10°C / min, and keeping warm for 30 minutes, then quickly cooling to 300°C, cooling naturally at room temperature, and cooling to room temperature; crushing the calcined powder to 800 mesh to obtain product 5, i.e., powder filler. The whiteness of the powder after calcination is 90.

[0032] Step 6. Prepare an additive C solution, add it to product 5, stir and blend to obtain a filler; in the filler, the additive C solution accounts for 3wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan; in the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan is 3:1:2; anhydrous ethanol is also added to the additive C solution during mixing, and the mass ratio of the additive C solution to anhydrous ethanol is 1:1.

[0033] Step 7. Place the mixed filler in a high-speed mixer and stir at 105°C for 1 hour; extrusion blend the filler at 60% and the matrix resin at 40% to prepare a coal gangue masterbatch. The matrix resin is PP-maleic anhydride (PP-g-MAH).

[0034] Step 8. Select the above masterbatch: ABS resin = 20wt%: 80wt% to prepare a high wear-resistant and high-temperature resistant mining equipment lining.

[0035] The liner prepared in this embodiment has a thermal deformation temperature of 103° C. and a mass wear of 0.403 g.

[0036] Example 2

[0037] Raw materials: coal gangue from a certain region, quartz content is 50wt%, clay content is 25wt%.

[0038] Preparation process of lining plate for mineral processing equipment in this embodiment:

[0039] Step 1. Pre-treat and crush the gangue to a particle size of D50≤30mm after crushing;

[0040] Step 2. Put the crushed coal gangue into a fluidized bed jet mill, add 5wt% of additive A, and perform a crushing operation by adjusting the classifying wheel. Product 1 is obtained at the discharge port, and product 2 is obtained in the dust removal bag; wherein the additive is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:2:2:3;

[0041] Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0042] Step 4. Mix product 2 and product 3 and grind them twice to obtain a powder with a D97 of 18 μm, i.e., product 4;

[0043] Step 5. Add 5wt% of additive B to product 4, where additive B is a mixture of sodium chloride, boric acid and magnesium sulfate in a mass ratio of 5:2.5:0.2; calcine in stages using a muffle furnace, a rotary kiln or a microwave calcining furnace, wherein the first stage is heated to 350°C at a heating rate of 10°C / min and kept warm for 30 minutes; the second stage is heated to 750°C at a heating rate of 20°C / min and kept warm for 10 minutes; the third stage is heated to 900°C at a heating rate of 10°C / min and kept warm for 30 minutes, then quickly cooled to 300°C, cooled naturally at room temperature, and cooled to room temperature; the calcined powder is crushed to 800 meshes to obtain product 5, i.e., powder filler. The whiteness of the calcined powder is 92.

[0044] Step 6. Prepare an additive C solution, add it to product 5, stir and blend, and obtain a filler; in the filler, the additive C solution accounts for 3wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan; during mixing, anhydrous ethanol is added to the additive C solution for dilution, and the mass ratio of the additive C solution to anhydrous ethanol is 1:1. In the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan is 4:2:2.

[0045] Step 7. Put the mixed filler into a high-speed mixer and stir at 105°C for 1 hour; extrusion blend the filler at 60wt% and the matrix resin at 40wt% to prepare a coal gangue masterbatch. The matrix resin is PP-maleic anhydride (PP-g-MAH).

[0046] Step 8. Select the above masterbatch: ABS resin = 30wt%: 70wt% to prepare a high wear-resistant and high-temperature resistant mining equipment lining.

[0047] The liner prepared in this embodiment has a thermal deformation temperature of 105°C and a mass wear of 0.352g.

[0048] Comparative Example 1

[0049] The difference from Example 1 is that the composition of additive A during pulverization is ammonium chloride and sodium oleate, and the mass ratio of the two is 3:2.

[0050] Comparative Example 2

[0051] The difference from Example 1 is that during calcination, additive B is a mixture of sodium chloride and boric acid in a mass ratio of 3:1.

[0052] Comparative Example 3

[0053] The difference from Example 1 is that during calcination, the temperature is directly raised to 850°C at a heating rate of 10°C / min, kept at that temperature for 30 minutes, then quickly cooled to 300°C, and naturally cooled to room temperature at room temperature.

[0054] Comparative Example 4

[0055] The difference from Example 1 is that after calcination, the mixture is air-cooled instead of being rapidly cooled to 300° C., but is directly cooled naturally to room temperature at room temperature.

[0056]

[0057] The above description is only a detailed description of the present invention in combination with a specific preferred embodiment, but the present invention is not limited thereto. Without departing from the concept of the present invention, if it still falls within the technical scope, the technical solution of the present invention can be subjected to a variety of simple modifications such as several simple deductions or replacements, including the combination of various technical features in any other appropriate manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a lining plate for a highly wear-resistant and high-temperature resistant ore dressing equipment, characterized in that: The following steps are involved: Step 1: preparing coal gangue powder with low quartz content, wherein the quartz content of the coal gangue powder is 10%-20%; Step 2: calcining the gangue powder in stages; Step 3: using the product obtained in step 2 to prepare highly wear-resistant and high-temperature-resistant coal gangue masterbatch; Step 4: Blend the coal gangue masterbatch with ABS resin to prepare a highly wear-resistant and high-temperature resistant lining.

2. The preparation method according to claim 1, characterized in that: The step 1 comprises: Step 1.1: Pre-treating and crushing the coal gangue, wherein the particle size after crushing is D50≤20mm; the quartz content in the coal gangue is greater than 50%; Step 1.2: Add 0.2-5% of additive A to the crushed coal gangue, grind it with a jet mill, obtain product 1 at the discharge port, and obtain product 2 in the dust removal bag; Step 1.3: Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3; Step 1.4: Product 2 and Product 3 are mixed and then crushed again to obtain a powder with a D97 of 18 μm.

3. The preparation method according to claim 2, characterized in that: In step 1.2, the additive A is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1-2:1-2:0.5-3.

4. The preparation method according to claim 1, characterized in that: Step 2 comprises: adding 3-5% additive B to the gangue powder obtained in step 1, calcining in stages, and finally crushing to 800 meshes; the additive B is prepared by mixing sodium chloride, boric acid and magnesium sulfate in a mass ratio of 3-5:1-2.5:0.5-2.

5. The preparation method according to claim 4, characterized in that: The staged calcination parameters are as follows: the first stage is heated from room temperature to 350°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes; the second stage is heated to 750°C, the heating rate is 20°C / min, and the temperature is kept for 10 minutes; the third stage is heated to 850-900°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes, and then quenched to 300°C, and then naturally cooled to room temperature.

6. The preparation method according to claim 1, characterized in that: Step 3 includes: Step 3.1: Add the additive C solution to the product obtained in step 2, stir and blend to obtain a filler; in the filler, the additive C solution accounts for 3-6wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan; in the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan is 3-4:1-2:1-2. Step 3.2: Extrusion blend the filler obtained in step 3.1 at a ratio of 60% filler and 40% matrix resin to prepare coal gangue masterbatch.

7. The preparation method according to claim 6, characterized in that: The filler mixed in step 3.1 was first stirred at 105° C. for 1 hour, and then the mixed filler was extruded and blended with the matrix resin.

8. The method according to claim 7, characterized in that In step 3.2, the base resin is PP-maleic anhydride or ABS.

9. The preparation method according to claim 1, characterized in that: In step 4, the mass ratio of the coal gangue masterbatch and the ABS resin is 20-30%:70-80%.

10. The preparation method according to claim 1, characterized in that: The thermal deformation temperature of the liner prepared in step 4 is 103-105°C.