Composite board and preparation method thereof
By preparing a composite treatment of high-toughness epoxy resin, modified carbon fiber and hydroxylated glass fiber, the problem of insufficient strength and toughness of composite boards was solved, and the comprehensive performance improvement of high strength, high toughness and corrosion resistance was achieved.
Patent Information
- Application Number
- CN202411184384.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing composite panels cannot simultaneously possess both high strength and high toughness, and their corrosion resistance is insufficient, making it difficult to meet the stringent performance requirements of aerospace, construction, and other fields.
A high-toughness epoxy resin component was prepared using adipic acid and epichlorohydrin, a toughening and modifying component was prepared using polyethylene glycol monomethyl ether and toluene diisocyanate, a carbon fiber was modified with magnesium nitrate hexahydrate, glass fiber was hydroxylated, and modified with silane coupling agent to form a stable three-dimensional mesh structure and interfacial bonding force, thereby improving the overall performance of the composite material.
The prepared composite plate, while maintaining high strength and high toughness, significantly improves corrosion resistance and is suitable for extreme working conditions and corrosive environments.
Smart Images

Figure BDA0005013120290000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a composite board and a preparation method thereof. Background Art
[0002] In the field of materials science, composite panels have attracted widespread attention due to their excellent comprehensive performance, especially in industrial applications with high requirements for material strength, toughness and corrosion resistance, such as aerospace, construction, chemical industry and other fields. Traditional materials are often difficult to meet these complex and stringent performance requirements. Therefore, it is particularly important to develop a composite panel with high strength, high toughness and corrosion resistance.
[0003] The strength and toughness of composite plates are one of their core performance indicators. Although traditional materials such as steel and aluminum alloys have high strength, they are often insufficient in toughness, especially prone to brittle fracture under extreme working conditions. Although polymer materials such as epoxy resins have good toughness, their strength is relatively low, which limits their application in high-demand situations. Therefore, how to develop composite plates with excellent corrosion resistance has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0004] Technical issues solved
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a composite plate and a preparation method thereof, which can effectively solve the problem that the composite plate of the prior art cannot have the characteristics of high strength and high toughness at the same time.
[0006] Technical Solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for preparing a composite plate, the preparation method comprising:
[0009] S1, using adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, then using polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials to prepare a toughening modification component, and finally modifying the carbon fiber with magnesium nitrate hexahydrate to prepare a modified carbon fiber component;
[0010] S2, modifying the high toughness epoxy resin component with a toughening modification component, a modified carbon fiber component, and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and the obtained component is recorded as a modified epoxy resin component;
[0011] S3, hydroxylating the glass fiber to prepare hydroxylated glass fiber, and evenly spraying the silane coupling agent solution on the surface of the hydroxylated glass fiber, the obtained solution is recorded as the glass fiber component;
[0012] S4. Add 10-15% by weight of diethylenetriamine and 35-40% by weight of glass fiber component to the modified epoxy resin component, stir at a stirring speed of 200 r / min for 1 min, pour into a mold and cure to obtain a composite board.
[0013] Furthermore, in S1, the preparation method of the high-toughness epoxy resin component is:
[0014] 0.1 mol adipic acid, 1.2 mol epichlorohydrin and 1 mmol benzyltriethylammonium chloride were weighed according to the calculated amount and added into a flask, and then placed in a water bath at 95°C for reaction for 2 hours. Then 1 g sodium hydroxide powder was added every 15 minutes, and added 8 times in total. Then the mixture was kept at the original water bath temperature for 3 hours. After the reaction was completed, it was filtered while hot and finally placed in a flask for rotary evaporation at 125°C for 30 minutes. The result was a high-toughness epoxy resin component.
[0015] Furthermore, in S1, the preparation method of the toughening and modifying component is:
[0016] Weigh calculated amounts of polyethylene glycol monomethyl ether and toluene diisocyanate in equimolar ratios for later use; add polyethylene glycol monomethyl ether into a flask, remove water in vacuo at 115°C for 3 hours, then cool to 40°C; then add toluene diisocyanate under stirring at a speed of 300 r / min; during the addition process, cool and control the temperature so that it is below 50°C; react for 2 hours, then heat to 75°C and react at a constant temperature for 1 hour to obtain the toughening modified component.
[0017] Furthermore, in S1, the preparation method of the modified carbon fiber component is:
[0018] S4.1. Soak the carbon fiber in acetone for 24 hours, then use anhydrous ethanol to ultrasonically clean it 5 times, then place it in an oven at 75°C to dry for 6 hours, then weigh 5g of it and soak it in nitric acid solution, place the soaked system in a water bath at 48°C and heat it for 10 minutes, wash it with deionized water 3 times after the soaking, and dry it. The result is recorded as the pretreated carbon fiber component;
[0019] S4.2. Soak the pretreated carbon fiber component in a tannic acid ethanol solution for 10 minutes, then soak it in a magnesium nitrate hexahydrate solution and vacuum infiltrate it for 2 hours to carry out a coating reaction. After the reaction is completed, place it on a rotary evaporator at 78°C for 2 hours, and dry it again to obtain the modified carbon fiber component.
[0020] Furthermore, in S4.1, the volume fraction of the nitric acid solution is 30%, and the drying method is to place it in an oven at 100°C and dry it for 2 hours. In S4.2, the concentration of the tannic acid ethanol solution is 3 g / L, and the concentration of the magnesium nitrate hexahydrate solution is 0.5 mol / L, and the drying method is to place it in an oven at 58°C and dry it to constant weight.
[0021] Furthermore, in S2, the preparation method of the modified epoxy resin component is: weigh 100g of high-toughness epoxy resin component and pour it into a flask, stir it at a stirring speed of 200r / min for 20min in a water bath at 90°C, heat it to 150°C, add 5g of toughening modification component, 12g of modified carbon fiber component and 18g of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, stir the reaction at the original stirring speed for 20min under nitrogen protection, heat it to 190°C, add 1g of triphenylphosphine and keep it warm for 3h, and the result is the modified epoxy resin component.
[0022] Furthermore, in S3, the hydroxylation treatment method is: soak the glass fiber in anhydrous ethanol for 12 hours, rinse it with deionized water for 3 times after soaking and enter it into a hydrochloric acid solution with a concentration of 0.5 mol / L, keep it at 80°C for 8 hours during the soaking process, then rinse it with deionized water until it is neutral and dry it in an oven at 42°C for 12 hours, and the result is hydroxylated glass fiber.
[0023] Furthermore, in S3, the preparation method of the silane coupling agent solution is: weigh 5-6g of silane coupling agent KH-560 and add it to 100g of deionized water, stir at a stirring speed of 300r / min for 10min, and then ultrasonically disperse at a frequency of 28kHz for 10min to obtain a silane coupling agent solution.
[0024] Furthermore, in S4, the curing treatment method is: first place it in an oven at 85°C for curing for 10 hours, and then place it at room temperature for 24 hours after demoulding.
[0025] A composite board is prepared by a composite board preparation method.
[0026] Beneficial Effects
[0027] The present invention provides a composite plate and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. The present invention uses adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, which can introduce flexible segments into the molecular chain of the epoxy resin through a two-step reaction of ring opening and ring closing, and can enhance the toughness of the epoxy resin; secondly, the toughening and modifying component prepared with polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials is an isocyanate prepolymer, which can react with hydroxyl groups to generate stable chemical bonds, thereby stably grafting it between the epoxy resin and the hydroxylated glass fiber, and can form a stable three-dimensional grid structure, so that the prepared composite material has the characteristics of high strength and high toughness.
[0029] 2. The present invention modifies the carbon fiber with magnesium nitrate hexahydrate to make the surface of the carbon fiber wrapped with magnesium oxide. Adding it to the preparation of the composite board can improve the interfacial bonding force between the carbon fiber and the epoxy resin matrix, and improve the overall mechanical properties of the composite board; secondly, the magnesium oxide layer serves as a protective layer, which can effectively isolate the carbon fiber from direct contact with oxygen in the air, delay the oxidation process of the carbon fiber, and improve its oxidation resistance. Moreover, in a corrosive environment, the magnesium oxide layer can serve as a barrier to slow down or prevent the corrosive medium from eroding the inside of the composite board, thereby improving its corrosion resistance.
[0030] 3. The hydroxylation treatment of the glass fiber in the present invention can generate hydroxyl groups on the surface of the glass fiber, which can improve the compatibility between the glass fiber and the epoxy resin matrix, so that the hydroxylated glass fiber can be more evenly dispersed in the modified epoxy resin component, which can improve the mechanical properties of the composite board; secondly, the hydroxylation treatment can change the chemical properties of the glass fiber surface, making it more corrosion-resistant, and combined with the corrosion resistance of the epoxy resin itself, the combination of the two can further improve the corrosion resistance of the composite board. The composite board prepared by the present invention has good corrosion resistance on the basis of high strength and toughness. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention will be further described below in conjunction with the embodiments.
[0033] Example 1
[0034] A method for preparing a composite plate in this embodiment is as follows:
[0035] S1, using adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, then using polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials to prepare a toughening modification component, and finally modifying the carbon fiber with magnesium nitrate hexahydrate to prepare a modified carbon fiber component;
[0036] Wherein, the preparation method of high toughness epoxy resin component is:
[0037] 0.1 mol adipic acid, 1.2 mol epichlorohydrin and 1 mmol benzyltriethylammonium chloride were weighed according to the calculated amount and added into a flask, and then placed in a water bath at 95°C for reaction for 2 hours. Then 1 g sodium hydroxide powder was added every 15 minutes, and added 8 times in total. Then the mixture was kept at the original water bath temperature for 3 hours. After the reaction was completed, it was filtered while hot and finally placed in a flask for rotary evaporation at 125°C for 30 minutes. The result was a high-toughness epoxy resin component.
[0038] The preparation method of the toughening and modifying component is as follows:
[0039] Weigh calculated amounts of polyethylene glycol monomethyl ether and toluene diisocyanate in equimolar ratios for later use; add polyethylene glycol monomethyl ether into a flask, remove water in vacuo at 115°C for 3 hours, then cool to 40°C; then add toluene diisocyanate under stirring at a speed of 300 r / min; during the addition process, cool and control the temperature so that it is below 50°C; react for 2 hours, then heat to 75°C and react at a constant temperature for 1 hour to obtain the toughening modified component.
[0040] The preparation method of the modified carbon fiber component is:
[0041] S4.1. Soak the carbon fiber in acetone for 24 hours, then use anhydrous ethanol to ultrasonically clean it 5 times, then place it in an oven at 75°C to dry it for 6 hours, then weigh 5g of it and soak it in a 30% nitric acid solution by volume, place the soaked system in a water bath at 48°C and heat it for 10 minutes, wash it with deionized water 3 times after the soaking, and place it in an oven at 100°C to dry it for 2 hours, and the result is recorded as the pretreated carbon fiber component;
[0042] S4.2. Soak the pretreated carbon fiber component in a 3 g / L tannic acid ethanol solution for 10 minutes, then soak it in a 0.5 mol / L magnesium nitrate hexahydrate solution and vacuum infiltrate it for 2 hours to carry out coating reaction. After the reaction is completed, place it at 78°C for 2 hours and place it in an oven at 58°C to dry to constant weight to obtain the modified carbon fiber component.
[0043] S2, modifying the high toughness epoxy resin component with a toughening modification component, a modified carbon fiber component, and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and the obtained component is recorded as a modified epoxy resin component;
[0044] Among them, the preparation method of the modified epoxy resin component is: weigh 100g of the high-toughness epoxy resin component and pour it into a flask, stir it at a stirring speed of 200r / min for 20min in a water bath at 90°C, heat it to 150°C, add 5g of the toughening modification component, 12g of the modified carbon fiber component and 18g of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, stir the reaction at the original stirring speed for 20min under nitrogen protection, heat it to 190°C, add 1g of triphenylphosphine and keep it warm for 3h, and the result is the modified epoxy resin component.
[0045] S3, hydroxylating the glass fiber to prepare hydroxylated glass fiber, and evenly spraying the silane coupling agent solution on the surface of the hydroxylated glass fiber, the obtained solution is recorded as the glass fiber component;
[0046] Among them, the method of hydroxylation treatment is: soak the glass fiber in anhydrous ethanol for 12 hours, rinse it with deionized water for 3 times after soaking and put it into a hydrochloric acid solution with a concentration of 0.5 mol / L, keep it at 80°C for 8 hours during the soaking process, then rinse it with deionized water until it is neutral and dry it in an oven at 42°C for 12 hours, and the result is hydroxylated glass fiber.
[0047] The preparation method of the silane coupling agent solution is as follows: weigh 5 g of silane coupling agent KH-560 and add it into 100 g of deionized water, stir at a stirring speed of 300 r / min for 10 min, and then ultrasonically disperse at a frequency of 28 kHz for 10 min to obtain the silane coupling agent solution.
[0048] S4, adding 10% by weight of diethylenetriamine and 35% by weight of glass fiber component to the modified epoxy resin component, stirring at a stirring speed of 200 r / min for 1 min, pouring into a mold and curing, and obtaining a composite board;
[0049] The curing method is as follows: firstly, the product is cured in an oven at 85°C for 10 hours, and then, after demoulding, the product is placed at room temperature for 24 hours.
[0050] A composite board is prepared by a composite board preparation method.
[0051] Example 2
[0052] A method for preparing a composite plate in this embodiment is as follows:
[0053] S1, using adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, then using polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials to prepare a toughening modification component, and finally modifying the carbon fiber with magnesium nitrate hexahydrate to prepare a modified carbon fiber component;
[0054] Wherein, the preparation method of high toughness epoxy resin component is:
[0055] 0.1 mol adipic acid, 1.2 mol epichlorohydrin and 1 mmol benzyltriethylammonium chloride were weighed according to the calculated amount and added into a flask, and then placed in a water bath at 95°C for reaction for 2 hours. Then 1 g sodium hydroxide powder was added every 15 minutes, and added 8 times in total. Then the mixture was kept at the original water bath temperature for 3 hours. After the reaction was completed, it was filtered while hot and finally placed in a flask for rotary evaporation at 125°C for 30 minutes. The result was a high-toughness epoxy resin component.
[0056] The preparation method of the toughening and modifying component is as follows:
[0057] Weigh calculated amounts of polyethylene glycol monomethyl ether and toluene diisocyanate in equimolar ratios for later use; add polyethylene glycol monomethyl ether into a flask, remove water in vacuo at 115°C for 3 hours, then cool to 40°C; then add toluene diisocyanate under stirring at a speed of 300 r / min; during the addition process, cool and control the temperature so that it is below 50°C; react for 2 hours, then heat to 75°C and react at a constant temperature for 1 hour to obtain the toughening modified component.
[0058] The preparation method of the modified carbon fiber component is:
[0059] S4.1. Soak the carbon fiber in acetone for 24 hours, then use anhydrous ethanol to ultrasonically clean it 5 times, then place it in an oven at 75°C to dry it for 6 hours, then weigh 5g of it and soak it in a 30% nitric acid solution by volume, place the soaked system in a water bath at 48°C and heat it for 10 minutes, wash it with deionized water 3 times after the soaking, and place it in an oven at 100°C to dry it for 2 hours, and the result is recorded as the pretreated carbon fiber component;
[0060] S4.2. Soak the pretreated carbon fiber component in a 3 g / L tannic acid ethanol solution for 10 minutes, then soak it in a 0.5 mol / L magnesium nitrate hexahydrate solution and vacuum infiltrate it for 2 hours to carry out coating reaction. After the reaction is completed, place it at 78°C for 2 hours and place it in an oven at 58°C to dry to constant weight to obtain the modified carbon fiber component.
[0061] S2, modifying the high toughness epoxy resin component with a toughening modification component, a modified carbon fiber component, and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and the obtained component is recorded as a modified epoxy resin component;
[0062] Among them, the preparation method of the modified epoxy resin component is: weigh 100g of the high-toughness epoxy resin component and pour it into a flask, stir it at a stirring speed of 200r / min for 20min in a water bath at 90°C, heat it to 150°C, add 5g of the toughening modification component, 12g of the modified carbon fiber component and 18g of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, stir the reaction at the original stirring speed for 20min under nitrogen protection, heat it to 190°C, add 1g of triphenylphosphine and keep it warm for 3h, and the result is the modified epoxy resin component.
[0063] S3, hydroxylating the glass fiber to prepare hydroxylated glass fiber, and evenly spraying the silane coupling agent solution on the surface of the hydroxylated glass fiber, the obtained solution is recorded as the glass fiber component;
[0064] Among them, the method of hydroxylation treatment is: soak the glass fiber in anhydrous ethanol for 12 hours, rinse it with deionized water for 3 times after soaking and put it into a hydrochloric acid solution with a concentration of 0.5 mol / L, keep it at 80°C for 8 hours during the soaking process, then rinse it with deionized water until it is neutral and dry it in an oven at 42°C for 12 hours, and the result is hydroxylated glass fiber.
[0065] The preparation method of the silane coupling agent solution is as follows: weigh 6 g of silane coupling agent KH-560 and add it into 100 g of deionized water, stir at a stirring speed of 300 r / min for 10 min, and then ultrasonically disperse at a frequency of 28 kHz for 10 min to obtain the silane coupling agent solution.
[0066] S4, adding 15% by weight of diethylenetriamine and 40% by weight of glass fiber component to the modified epoxy resin component, stirring at a stirring speed of 200 r / min for 1 min, pouring into a mold and curing, and obtaining a composite board;
[0067] The curing method is as follows: firstly, the product is cured in an oven at 85°C for 10 hours, and then, after demoulding, the product is placed at room temperature for 24 hours.
[0068] A composite board is prepared by a composite board preparation method.
[0069] Example 3
[0070] A method for preparing a composite plate in this embodiment is as follows:
[0071] S1, using adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, then using polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials to prepare a toughening modification component, and finally modifying the carbon fiber with magnesium nitrate hexahydrate to prepare a modified carbon fiber component;
[0072] Wherein, the preparation method of high toughness epoxy resin component is:
[0073] 0.1 mol adipic acid, 1.2 mol epichlorohydrin and 1 mmol benzyltriethylammonium chloride were weighed according to the calculated amount and added into a flask, and then placed in a water bath at 95°C for reaction for 2 hours. Then 1 g sodium hydroxide powder was added every 15 minutes, and added 8 times in total. Then the mixture was kept at the original water bath temperature for 3 hours. After the reaction was completed, it was filtered while hot and finally placed in a flask for rotary evaporation at 125°C for 30 minutes. The result was a high-toughness epoxy resin component.
[0074] The preparation method of the toughening and modifying component is as follows:
[0075] Weigh calculated amounts of polyethylene glycol monomethyl ether and toluene diisocyanate in equimolar ratios for later use; add polyethylene glycol monomethyl ether into a flask, remove water in vacuo at 115°C for 3 hours, then cool to 40°C; then add toluene diisocyanate under stirring at a speed of 300 r / min; during the addition process, cool and control the temperature so that it is below 50°C; react for 2 hours, then heat to 75°C and react at a constant temperature for 1 hour to obtain the toughening modified component.
[0076] The preparation method of the modified carbon fiber component is:
[0077] S4.1. Soak the carbon fiber in acetone for 24 hours, then use anhydrous ethanol to ultrasonically clean it 5 times, then place it in an oven at 75°C to dry it for 6 hours, then weigh 5g of it and soak it in a 30% nitric acid solution by volume, place the soaked system in a water bath at 48°C and heat it for 10 minutes, wash it with deionized water 3 times after the soaking, and place it in an oven at 100°C to dry it for 2 hours, and the result is recorded as the pretreated carbon fiber component;
[0078] S4.2. Soak the pretreated carbon fiber component in a 3 g / L tannic acid ethanol solution for 10 minutes, then soak it in a 0.5 mol / L magnesium nitrate hexahydrate solution and vacuum infiltrate it for 2 hours to carry out coating reaction. After the reaction is completed, place it at 78°C for 2 hours and place it in an oven at 58°C to dry to constant weight to obtain the modified carbon fiber component.
[0079] S2, modifying the high toughness epoxy resin component with a toughening modification component, a modified carbon fiber component, and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and the obtained component is recorded as a modified epoxy resin component;
[0080] Among them, the preparation method of the modified epoxy resin component is: weigh 100g of the high-toughness epoxy resin component and pour it into a flask, stir it at a stirring speed of 200r / min for 20min in a water bath at 90°C, heat it to 150°C, add 5g of the toughening modification component, 12g of the modified carbon fiber component and 18g of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, stir the reaction at the original stirring speed for 20min under nitrogen protection, heat it to 190°C, add 1g of triphenylphosphine and keep it warm for 3h, and the result is the modified epoxy resin component.
[0081] S3, hydroxylating the glass fiber to prepare hydroxylated glass fiber, and evenly spraying the silane coupling agent solution on the surface of the hydroxylated glass fiber, the obtained solution is recorded as the glass fiber component;
[0082] Among them, the method of hydroxylation treatment is: soak the glass fiber in anhydrous ethanol for 12 hours, rinse it with deionized water for 3 times after soaking and put it into a hydrochloric acid solution with a concentration of 0.5 mol / L, keep it at 80°C for 8 hours during the soaking process, then rinse it with deionized water until it is neutral and dry it in an oven at 42°C for 12 hours, and the result is hydroxylated glass fiber.
[0083] The preparation method of the silane coupling agent solution is as follows: weigh 6 g of silane coupling agent KH-560 and add it into 100 g of deionized water, stir at a stirring speed of 300 r / min for 10 min, and then ultrasonically disperse at a frequency of 28 kHz for 10 min to obtain the silane coupling agent solution.
[0084] S4, adding 13% by weight of diethylenetriamine and 38% by weight of glass fiber component to the modified epoxy resin component, stirring at a stirring speed of 200 r / min for 1 min, pouring into a mold and curing, and obtaining a composite board;
[0085] The curing method is as follows: firstly, the product is cured in an oven at 85°C for 10 hours, and then, after demoulding, the product is placed at room temperature for 24 hours.
[0086] A composite board is prepared by a composite board preparation method.
[0087] Comparative Example 1
[0088] The composite board and preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the high-toughness epoxy resin component in Example 1 is replaced with commercially available E-51 epoxy resin.
[0089] Comparative Example 2
[0090] The composite board and preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the modified carbon fiber component in Example 1 is replaced with unmodified carbon fiber.
[0091] Comparative Example 3
[0092] The composite board and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the hydroxylated glass fiber in Example 1 is replaced with glass fiber that has not been subjected to hydroxylation treatment.
[0093] Performance Testing
[0094] The composite plates in Examples 1-3 and Comparative Examples 1-3 are marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-3 is tested. The specific test items and test methods are as follows:
[0095] 1. The tensile strength and elongation at break of Examples 1-3 and Comparative Examples 1-3 were tested according to the testing method of GB / T2567-2021, and the obtained data are recorded in the following table;
[0096] 2. The impact strength of Examples 1-3 and Comparative Examples 1-3 was tested according to the GB / T2571-2021 test method, and the obtained data are recorded in the following table;
[0097] 3. Embodiments 1-3 and comparative examples 1-3 were respectively immersed in a 3% hydrochloric acid solution and a 3% sodium hydroxide solution at 25°C for 24 hours. If there was no wrinkling, blistering, discoloration, etc. on the surface, it indicated that the corrosion resistance was excellent. If there were wrinkling, blistering, discoloration, etc., it indicated that the corrosion resistance was average. The obtained data are recorded in the following table.
[0098]
[0099] It can be seen from the data in the above table that the tensile strength, elongation at break and impact strength of the composite plates in Examples 1-3 are significantly better than those in Comparative Examples 1-3, indicating that the high-toughness epoxy resin component, modified carbon fiber component and hydroxylated glass fiber added in the preparation of the composite plates can be matched with each other, thereby improving the mechanical properties of the composite plates. The corrosion resistance of the composite plates in Examples 1-3 is significantly better than that in Comparative Examples 2-3, indicating that the modified carbon fiber component and hydroxylated glass fiber added in the preparation of the composite plates can play a role in improving the corrosion resistance.
[0100] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0101] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a composite plate, It is characterized in that The preparation method is: S1, using adipic acid and epichlorohydrin as raw materials to prepare a high-toughness epoxy resin component, then using polyethylene glycol monomethyl ether and toluene diisocyanate as raw materials to prepare a toughening modification component, and finally modifying the carbon fiber with magnesium nitrate hexahydrate to prepare a modified carbon fiber component; S2, modifying the high toughness epoxy resin component with a toughening modification component, a modified carbon fiber component, and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and the obtained component is recorded as a modified epoxy resin component; S3, hydroxylating the glass fiber to prepare hydroxylated glass fiber, and evenly spraying the silane coupling agent solution on the surface of the hydroxylated glass fiber, the obtained solution is recorded as the glass fiber component; S4. Add 10-15% by weight of diethylenetriamine and 35-40% by weight of glass fiber component to the modified epoxy resin component, stir at a stirring speed of 200 r / min for 1 min, pour into a mold and cure to obtain a composite board.
2. A method for preparing a composite board according to claim 1, It is characterized in that In S1, the preparation method of the high-toughness epoxy resin component is: 0.1 mol of adipic acid, 1.2 mol of epichlorohydrin and 1 mmol of benzyltriethylammonium chloride were weighed according to the calculated amount and added into a flask, and then placed in a water bath at 95°C for reaction for 2 hours. Then, 1 g of sodium hydroxide powder was added every 15 minutes, and added 8 times in total. Then, the reaction was kept at the original water bath temperature for 3 hours. After the reaction was completed, it was filtered while hot, and finally placed in a flask at 125°C for rotary evaporation for 30 minutes. The result was a high-toughness epoxy resin component.
3. A method for preparing a composite board according to claim 1, It is characterized in that In S1, the preparation method of the toughening and modifying component is: Weigh calculated amounts of polyethylene glycol monomethyl ether and toluene diisocyanate in equimolar ratios for later use; add polyethylene glycol monomethyl ether into a flask, remove water in vacuo at 115°C for 3 hours, then cool to 40°C; then add toluene diisocyanate under stirring at a speed of 300 r / min; during the addition process, cool and control the temperature so that it is below 50°C; react for 2 hours, then heat to 75°C and react at a constant temperature for 1 hour to obtain the toughening modified component.
4. The method for preparing a composite board according to claim 1, It is characterized in that In S1, the preparation method of the modified carbon fiber component is: S4.
1. Soak the carbon fiber in acetone for 24 hours, then use anhydrous ethanol to ultrasonically clean it 5 times, then place it in an oven at 75°C to dry for 6 hours, then weigh 5g of it and soak it in nitric acid solution, place the soaked system in a water bath at 48°C and heat it for 10 minutes, wash it with deionized water 3 times after the soaking, and dry it. The result is recorded as the pretreated carbon fiber component; S4.
2. Soak the pretreated carbon fiber component in a tannic acid ethanol solution for 10 minutes, then soak it in a magnesium nitrate hexahydrate solution and vacuum infiltrate it for 2 hours to carry out a coating reaction. After the reaction is completed, place it on a rotary evaporator at 78°C for 2 hours, and dry it again to obtain the modified carbon fiber component.
5. A method for preparing a composite board according to claim 4, It is characterized in that In S4.1, the volume fraction of the nitric acid solution is 30%, and the drying method is to place it in an oven at 100°C for 2 hours. In S4.2, the concentration of the tannic acid ethanol solution is 3 g / L, and the concentration of the magnesium nitrate hexahydrate solution is 0.5 mol / L. The drying method is to place it in an oven at 58°C to constant weight.
6. The method for preparing a composite board according to claim 1, It is characterized in that In S2, the preparation method of the modified epoxy resin component is as follows: weigh 100g of the high-toughness epoxy resin component and pour it into a flask, stir it at a stirring speed of 200r / min for 20min in a water bath at 90°C, heat it to 150°C, add 5g of the toughening modification component, 12g of the modified carbon fiber component and 18g of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, stir the reaction at the original stirring speed for 20min under nitrogen protection, heat it to 190°C, add 1g of triphenylphosphine and keep it warm for 3h, and the result is the modified epoxy resin component.
7. The method for preparing a composite board according to claim 1, It is characterized in that In S3, the hydroxylation treatment method is: soak the glass fiber in anhydrous ethanol for 12 hours, rinse it with deionized water for 3 times and put it into a hydrochloric acid solution with a concentration of 0.5 mol / L, keep it at 80°C for 8 hours during the soaking process, then rinse it with deionized water until it is neutral and dry it in an oven at 42°C for 12 hours, and the result is hydroxylated glass fiber.
8. The method for preparing a composite board according to claim 1, It is characterized in that In S3, the preparation method of the silane coupling agent solution is: weigh 5-6g of silane coupling agent KH-560 and add it into 100g of deionized water, stir at a stirring speed of 300r / min for 10min, and then ultrasonically disperse at a frequency of 28kHz for 10min to obtain the silane coupling agent solution.
9. The method for preparing a composite board according to claim 1, It is characterized in that In S4, the curing treatment method is: first place in an oven at 85°C for curing for 10 hours, and then place at room temperature for 24 hours after demoulding.
10. A composite board, It is characterized in that The composite board is prepared by the method for preparing the composite board according to any one of claims 1 to 9.
Citation Information
Patent Citations
Curable epoxy resin compositions and composites made therefrom
CN104271667A
Preparation method of impact-resistant high-toughness carbon fiber composite material
CN105670287A
Carbon fiber reinforced resin based high-performance light composite material and preparation method thereof
CN107936273A
Carbon fiber and glass fiber mixed composite tube and preparation method thereof
CN108036123A
Method for preparing reinforced phenolic aldehyde-epoxy resin composite material by utilizing hollow glass bead-carbon fiber sheet-glass fiber
CN108976716A
Cited By
High-strength composite electric pole material and preparation method thereof
CN120025661A