Polyester film for MLCC high-smoothness release film and preparation method thereof

By adding silica and calcium carbonate to the polyester film, combined with the ratio and process of components such as flame retardant and slip agent, the problem of insufficient smoothness and peeling performance in MLCC manufacturing is solved, and the problem of traditional films is achieved. High precision and high quality MLCC manufacturing.

CN118931121AInactive Publication Date: 2024-11-12FOSHAN SAIHE FILM TECH CO LTD

Patent Information

Application Number
CN202411091342.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polyester films have problems such as insufficient smoothness, poor peeling performance, and difficult to take into account both weathering and processing performance in the application of MLCC release films, which limits the high precision and high quality development of MLCC manufacturing.

Method used

The ratio of polyester slices, silica, calcium carbonate, flame retardant, slip agent, toughener, antioxidant and ultraviolet absorber is adopted, and the ratio of high-speed mixing, melt extrusion, casting molding and wire coating are adopted. By processing, a polyester film with high smoothness, excellent peeling, weather resistance and processability was prepared.

Benefits of technology

It significantly improves the smoothness and comprehensive performance of the film, meets the strict standards of high-end MLCC manufacturing, reduces costs, and enhances the weather resistance and processing performance of the film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of polyester films, and discloses a polyester film for an MLCC high-smoothness release film and a preparation method thereof.The polyester film for the MLCC high-smoothness release film comprises, by weight, 75-90 parts of polyester chips, 3-5 parts of silicon dioxide, 10-15 parts of calcium carbonate, 3-8 parts of a flame retardant, 3-5 parts of a slip agent, 3-5 parts of a flexibilizer and 0.3-0.5 part of an antioxidant. 0.3-0.5 part of an ultraviolet light absorber; according to the invention, silicon dioxide and calcium carbonate are added as fillers, so that not only are the hardness and wear resistance of the film improved, but also the cost is reduced by reducing the use amount of polyester; in addition, through the synergistic effect of the flame retardant, the slip agent, the flexibilizer, the antioxidant and the ultraviolet light absorber, the weather resistance, the flame retardance, the processability and the long-term use stability of the film are further enhanced; the obtained polyester film has extremely high smoothness and is beneficial to improving the manufacturing precision and performance of the MLCC.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polyester films, and specifically relates to a polyester film for MLCC high-smooth release film and a preparation method thereof. Background Art

[0002] In the rapidly developing electronics industry, MLCC (chip multilayer ceramic capacitor) is a key component, and its performance directly affects the stability and reliability of the entire electronic system. When traditional polyester films are used in MLCC release films, they often face problems such as insufficient smoothness, poor peeling performance, and difficulty in balancing weather resistance and processing performance. These defects limit the high-precision and high-quality development of MLCC manufacturing. Therefore, the development of a polyester film with high smoothness, excellent peelability, good processability and stable weather resistance has become an urgent need in the industry. How to design a polyester film with a reasonable ratio to achieve high smoothness to meet the high-precision requirements of MLCC manufacturing, while having good peelability, weather resistance, processability and long-term use stability has become a technical problem that needs to be solved urgently. Specifically, the technical problems that need to be solved include: How to significantly improve the smoothness and comprehensive performance of the film through reasonable formula adjustment while maintaining the cost-effectiveness of the film to meet the stringent standards of high-end MLCC manufacturing. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a polyester film for MLCC high-smooth release film and a preparation method thereof, which effectively solves the problems raised by the background technology.

[0004] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a polyester film for MLCC high-smooth release film, comprising the following components in parts by weight: 75-90 parts of polyester chips, 3-5 parts of silicon dioxide, 10-15 parts of calcium carbonate, 3-8 parts of flame retardant, 3-5 parts of slip agent, 3-5 parts of toughening agent, 0.3-0.5 parts of antioxidant, and 0.3-0.5 parts of ultraviolet absorber.

[0005] Preferably, the composition comprises the following components in parts by weight: 76-85 parts of polyester chips, 4-5 parts of silicon dioxide, 11-14 parts of calcium carbonate, 4-7 parts of flame retardant, 3-4 parts of slip agent, 3-4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

[0006] Preferably, the composition comprises the following components in parts by weight: 80 parts of polyester chips, 4 parts of silicon dioxide, 13 parts of calcium carbonate, 5 parts of flame retardant, 3 parts of slip agent, 4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

[0007] Preferably, the flame retardant is aluminum hydroxide, the slip agent is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0008] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0009] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0010] Step 2: premix all the raw materials in a high-speed mixer;

[0011] Step three, melt extrusion: send into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone between 250°C and 280°C; maintain the die temperature of the extruder between 260°C and 270°C; adjust the screw speed of the extruder: set the screw speed between 30 and 80 rpm according to production requirements and equipment performance.

[0012] Step 4, tape casting: after the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted between 10 and 50 m / min; and the temperature of the cooling roller is adjusted to be between 20°C and 40°C;

[0013] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0014] Step 6: Drying: Send the coated film into a drying device and dry it at a temperature of 80°C to 120°C for 1 to 5 minutes.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] By adding silica and calcium carbonate as fillers, not only the hardness and wear resistance of the film are improved, but also the cost is reduced by reducing the use of polyester; in addition, the synergistic effect of flame retardants, lubricants, toughening agents, antioxidants and UV absorbers further enhances the film's weather resistance, flame retardancy, processing performance and long-term use stability; the obtained polyester film has extremely high smoothness, which is beneficial to improving the manufacturing accuracy and performance of MLCC. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0018] The invention relates to a polyester film for a high-smooth release film of MLCC, comprising the following components in parts by weight: 75-90 parts of polyester chips, 3-5 parts of silicon dioxide, 10-15 parts of calcium carbonate, 3-8 parts of flame retardants, 3-5 parts of slip agents, 3-5 parts of toughening agents, 0.3-0.5 parts of antioxidants, and 0.3-0.5 parts of ultraviolet absorbers.

[0019] The invention comprises the following components in parts by weight: 76-85 parts of polyester chips, 4-5 parts of silicon dioxide, 11-14 parts of calcium carbonate, 4-7 parts of flame retardant, 3-4 parts of lubricant, 3-4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

[0020] The invention comprises the following components in parts by weight: 80 parts of polyester chips, 4 parts of silicon dioxide, 13 parts of calcium carbonate, 5 parts of flame retardant, 3 parts of slip agent, 4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

[0021] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0022] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0023] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0024] Step 2: premix all the raw materials in a high-speed mixer;

[0025] Step three, melt extrusion: send into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone between 250°C and 280°C; maintain the die temperature of the extruder between 260°C and 270°C; adjust the screw speed of the extruder: set the screw speed between 30 and 80 rpm according to production requirements and equipment performance.

[0026] Step 4, tape casting: after the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted between 10 and 50 m / min; and the temperature of the cooling roller is adjusted to be between 20°C and 40°C;

[0027] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0028] Step 6: Drying: Send the coated film into a drying device and dry it at a temperature of 80°C to 120°C for 1 to 5 minutes.

[0029] Embodiment 1:

[0030] A polyester film for MLCC high-smooth release film comprises the following components in parts by weight: 75 parts of polyester chips, 3 parts of silicon dioxide, 10 parts of calcium carbonate, 3 parts of flame retardant, 3 parts of slip agent, 3 parts of toughening agent, 0.3 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0031] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0032] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0033] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0034] Step 2: premix all the raw materials in a high-speed mixer;

[0035] Step three, melt extrusion: send it into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone at 250°C; maintain the die temperature of the extruder at 260°C; adjust the screw speed of the extruder: set the screw speed at 30 / min according to production requirements and equipment performance.

[0036] Step 4, tape casting: After the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted to 10 m / min; and the temperature of the cooling roller is adjusted to set the cooling roller temperature at 20°C;

[0037] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0038] Step 6: Drying: Send the coated film into a drying device and dry it at 80°C for 5 minutes.

[0039] Embodiment 2:

[0040] A polyester film for MLCC high-smooth release film comprises the following components in parts by weight: 90 parts of polyester chips, 5 parts of silicon dioxide, 15 parts of calcium carbonate, 8 parts of flame retardant, 5 parts of slip agent, 5 parts of toughening agent, 0.5 parts of antioxidant, and 0.5 parts of ultraviolet absorber.

[0041] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0042] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0043] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0044] Step 2: premix all the raw materials in a high-speed mixer;

[0045] Step three, melt extrusion: send it into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone at 280°C; maintain the die temperature of the extruder at 270°C; adjust the screw speed of the extruder: set the screw speed at 80 rpm according to production requirements and equipment performance.

[0046] Step 4, tape casting: After the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted between 50 meters / minute; and the temperature of the cooling roller is adjusted to set the temperature of the cooling roller between 40°C;

[0047] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0048] Step 6: Drying: Send the coated film into a drying device and dry it at 120° C. for 1 minute.

[0049] Embodiment 3:

[0050] A polyester film for MLCC high-smooth release film comprises the following components in parts by weight: 80 parts of polyester chips, 4 parts of silicon dioxide, 13 parts of calcium carbonate, 5 parts of flame retardant, 3 parts of slip agent, 4 parts of toughening agent, 0.4 parts of antioxidant, and 0.4 parts of ultraviolet absorber.

[0051] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0052] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0053] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0054] Step 2: premix all the raw materials in a high-speed mixer;

[0055] Step three, melt extrusion: send it into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone at 270°C; maintain the die temperature of the extruder at 265°C; adjust the screw speed of the extruder: set the screw speed at 50 rpm according to production requirements and equipment performance.

[0056] Step 4, tape casting: After the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted to 30 m / min; and the temperature of the cooling roller is adjusted to set the cooling roller temperature at 30°C;

[0057] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0058] Step 6: Drying: Send the coated film into a drying device and dry it at 90°C for 3 minutes.

[0059] Embodiment 4:

[0060] A polyester film for MLCC high-smooth release film comprises the following components in parts by weight: 76 parts of polyester chips, 4 parts of silicon dioxide, 11 parts of calcium carbonate, 4 parts of flame retardant, 3 parts of slip agent, 3 parts of toughening agent, 0.4 parts of antioxidant, and 0.4 parts of ultraviolet absorber.

[0061] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0062] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0063] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0064] Step 2: premix all the raw materials in a high-speed mixer;

[0065] Step three, melt extrusion: send it into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone at 250°C; maintain the die temperature of the extruder at 260°C; adjust the screw speed of the extruder: set the screw speed at 30 rpm according to production requirements and equipment performance.

[0066] Step 4, tape casting: After the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted to 20 m / min; and the temperature of the cooling roller is adjusted to set the cooling roller temperature at 30°C;

[0067] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0068] Step 6: Drying: The coated film is sent to a drying device and dried at 100° C. for 2 minutes.

[0069] Embodiment 5:

[0070] A polyester film for MLCC high-smooth release film comprises the following components in parts by weight: 85 parts of polyester chips, 5 parts of silicon dioxide, 14 parts of calcium carbonate, 7 parts of flame retardant, 4 parts of slip agent, 4 parts of toughening agent, 0.4 parts of antioxidant, and 0.4 parts of ultraviolet absorber.

[0071] The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

[0072] A method for preparing a polyester film for a high-smooth release film for MLCC comprises the following steps:

[0073] Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio;

[0074] Step 2: premix all the raw materials in a high-speed mixer;

[0075] Step three, melt extrusion: send it into a twin-screw extruder for melt extrusion. The specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone at 250°C; maintain the die temperature of the extruder at 260°C; adjust the screw speed of the extruder: set the screw speed at 30 rpm according to production requirements and equipment performance.

[0076] Step 4, tape casting: After the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; according to the film thickness requirements, the tape casting speed is adjusted to 20 m / min; and the temperature of the cooling roller is adjusted to set the cooling roller temperature at 30°C;

[0077] Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed;

[0078] Step 6: Drying: The coated film is sent to a drying device and dried at 100° C. for 2 minutes.

[0079] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A polyester film for MLCC high smoothness release film, It is characterized in that The invention comprises the following components in parts by weight: 75-90 parts of polyester chips, 3-5 parts of silicon dioxide, 10-15 parts of calcium carbonate, 3-8 parts of flame retardant, 3-5 parts of slip agent, 3-5 parts of toughening agent, 0.3-0.5 parts of antioxidant and 0.3-0.5 parts of ultraviolet absorber.

2. The polyester film for MLCC high smoothness release film according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 76-85 parts of polyester chips, 4-5 parts of silicon dioxide, 11-14 parts of calcium carbonate, 4-7 parts of flame retardant, 3-4 parts of lubricant, 3-4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

3. The polyester film for MLCC high smoothness release film according to claim 2, It is characterized in that The invention comprises the following components in parts by weight: 80 parts of polyester chips, 4 parts of silicon dioxide, 13 parts of calcium carbonate, 5 parts of flame retardant, 3 parts of slip agent, 4 parts of toughening agent, 0.4 parts of antioxidant and 0.4 parts of ultraviolet absorber.

4. The polyester film for MLCC high smoothness release film according to claim 1, It is characterized in that The flame retardant is aluminum hydroxide, the lubricant is dimethyl silicone oil, the toughening agent is thermoplastic polyester elastomer, the antioxidant is dilauryl thiodipropionate, and the ultraviolet absorber is phenyl salicylate.

5. A method for preparing a polyester film for MLCC high-smooth release film according to claim 1, It is characterized in that The following steps are involved: Step 1, raw material preparation: prepare materials according to the ratio: accurately weigh and evenly mix the flame retardant, lubricant, toughening agent, antioxidant and ultraviolet absorber in sequence according to the ratio; Step 2: premix all the raw materials in a high-speed mixer; Step 3, melt extrusion: send it into a twin-screw extruder for melt extrusion, the specific process is: add the proportioned raw materials into the extruder, set the temperature of the heating zone between 250°C and 280°C; keep the die temperature of the extruder between 260°C and 270°C; adjust the screw speed of the extruder: according to production requirements and equipment performance, set the screw speed between 30 and 80 rpm; Step 4, tape casting: after the molten material flows out through the die head, it is evenly spread on the tape casting machine and cooled and solidified into a film; According to the film thickness requirements, adjust the casting speed between 10 and 50 m / min; And adjust the temperature of the cooling roller to set the temperature of the cooling roller between 20℃ and 40℃; Step 5, online coating: coating the functional coating on the film surface, the coating speed needs to match the casting speed; Step 6: Drying: Send the coated film into a drying device and dry it at a temperature of 80°C to 120°C for 1 to 5 minutes.

Citation Information

Patent Citations

  • Ultra-low surface roughness polyester base film / composite base film and preparation method thereof

    CN107915960A

  • Low-roughness release base film for MLCC process and preparation method of the low-roughness release base film

    CN111873587A

  • MLCC release film base film and preparation method thereof

    CN114407468A

  • Polyester master batch special for MLCC release film and preparation method of polyester master batch

    CN115322533A

  • High-temperature-resistant low-precipitation transparent polyester film and preparation method thereof

    CN116834414A

Cited By

  • Agricultural flame-retardant weather-resistant polyester film and preparation method thereof

    CN120795558A