TPEE foaming composite material as well as preparation method and application thereof

By filling TPEE resin with high temperature oil and introducing polyester fiber, the problems of TPEE foaming materials with poor hand feel and low foaming efficiency in soft interiors of automobiles are solved, and the effect of high foaming performance and good touch is achieved, avoiding The collapse of the holes meets the high foaming ratio and product appearance requirements of the soft interior of the car.

CN118931153APending Publication Date: 2024-11-12ORINKO ADVANCED PLASTICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411104428.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing TPEE foaming materials have defects such as high-hardness foaming effect but poor feel in automotive soft interior applications, low-hardness feel but low foaming efficiency, and are difficult to meet the requirements of high foaming ratio and good product appearance. It is easy to cause convergence of holes.

Method used

By filling TPEE resin with high temperature oil, introducing polyester fibers, and forming disordered network connections during chemical injection molding and molding foaming, avoiding melt pulling and rupture, and achieving material characteristics with high foaming thickness and low surface hardness.

Benefits of technology

It achieves high foaming performance, continuous sealing and collapse-free bubble cells, can perform large-distance mold opening, and obtain low hardness and good touch automotive soft interior materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990319660000061
    Figure BDA0004990319660000061
Patent Text Reader

Abstract

The invention discloses a TPEE foamed composite material as well as a preparation method and application thereof. The TPEE foaming composite material comprises the following raw materials: 50 to 80 parts of TPEE resin, 10 to 40 parts of plasticizing oil, 1 to 6 parts of polyester fiber, 0.5 to 3 parts of a coupling agent, 0.1 to 0.6 part of an antioxidant, 0.1 to 2 parts of a lubricant and 0.5 to 3 parts of other auxiliary agents. The plasticizing oil comprises one or more of paraffin oil, cycloalkane oil, aromatic hydrocarbon oil and straight-chain alkane oil; and the polyester fibers are chopped fibers. According to the TPEE foaming material, TPEE resin is heated and filled with oil, the initial hardness of the material is greatly reduced, the mold opening distance is controlled in the injection molding process, different product thicknesses are achieved, disordered network connection is formed between TPEE foaming melts by introducing polyester fibers, the melts are prevented from being pulled and broken in the mold opening process, and a foaming sandwich structure which is uniform in foam holes and free of large-area collapse is obtained. And the composite material has the characteristics of ultra-low hardness and skin-friendly touch feeling, and can be widely applied to soft interior parts of automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and specifically relates to a TPEE foaming composite material, a preparation method and an application thereof. Background Art

[0002] Thermoplastic polyether ester elastomer is a type of copolymer polymer material with physical properties between thermosetting rubber and thermoplastic plastics, also known as polyether ester synthetic rubber. It has both the elasticity of rubber and the processability of plastics, and can be recycled and reprocessed without significant loss of product performance. TPEE has good weather resistance, ozone resistance, UV resistance and impact resistance, and can be molded and processed by ordinary thermoplastic plastic processing equipment and is reusable. It is replacing some thermosetting vulcanized rubber materials and slush PVC materials, and is widely used in automotive, electrical and electronic, industrial and civil fields.

[0003] TPEE foaming is also an effective means to expand the application of TPEE materials. Through certain process methods, a uniform and dense pore structure is produced inside the TPEE material, which makes it have the high mechanical strength and resilience of TPEE as well as the stress absorption, buffering and shock absorption properties of foaming materials, and can effectively absorb the energy generated by extrusion and impact during use. Thermoplastic polyester elastomer foaming material is an excellent damping, shock absorption, heat insulation and sound insulation material with broad application prospects.

[0004] At present, most TPEE has the characteristics of low melt viscosity and low melt strength. In the application scenario of soft automotive interior, under the injection molding chemical foaming process, high-hardness TPEE has better foaming effect but poor hand feel, low-hardness TPEE has slightly better hand feel but poor foaming efficiency, low ratio, and easy to produce defects such as pore collapse. It is difficult to meet the requirements of high foaming ratio, good product appearance, and ultra-low hardness and good touch required by automotive soft interior materials. Summary of the invention

[0005] The present invention provides a TPEE foam composite material, a preparation method and an application thereof, which greatly reduces the initial hardness of the TPEE material by oil-filling the TPEE resin at high temperature, further introduces polyester fibers, and forms a disordered network connection between the TPEE foam melts in the subsequent chemical injection molding and mold opening foaming process to avoid the melt pulling and rupture, so that it maintains continuous bubbles, and avoids the drawbacks of further reducing the melt strength of the TPEE material and deteriorating the foaming performance due to the oil-filled plasticizer. It can perform a large-distance mold opening action to achieve a good touch material with high foaming thickness and low surface hardness.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A TPEE foam composite material, comprising the following raw materials:

[0008] TPEE resin 50-80 parts, plasticizer oil 10-40 parts, polyester fiber 1-6 parts, coupling agent 0.5-3 parts, antioxidant 0.1-0.6 parts, lubricant 0.1-2 parts, chemical foaming agent 0.5-5 parts and auxiliary agent 0-3 parts;

[0009] The plasticizing oil includes one or more of paraffin oil, cycloparaffin oil, aromatic hydrocarbon oil and straight-chain paraffin oil;

[0010] The polyester fibers are short-cut fibers.

[0011] Preferably, the TPEE resin has a hardness of 25D to 75D.

[0012] Preferably, the chemical foaming agent comprises NaHCO 3 and one or more of azodicarbonamide.

[0013] Preferably, the antioxidant includes one or more of hindered phenol, thioester and phosphite antioxidants.

[0014] Preferably, the lubricant includes one or more of erucamide, calcium stearate, stearic acid amide, silicone masterbatch and polyethylene wax.

[0015] Preferably, the coupling agent includes one or more of KH550 and KH560.

[0016] Preferably, the auxiliary agent includes one or more of an ultraviolet light absorber, a light stabilizer, an antistatic agent and a colorant.

[0017] A method for preparing a TPEE foamed composite material comprises the following steps:

[0018] Spraying a coupling agent on the surface of the polyester fiber, wherein the mass ratio of the polyester fiber to the coupling agent is 2:1, to obtain a pretreated polyester fiber;

[0019] Heat and mix 50-80 parts of TPEE resin and 10-40 parts of plasticizer oil, and stir to make TPEE swell and absorb the plasticizer oil until there is no plasticizer oil residue in the stirring pot and on the surface of TPEE resin, thus completing the oil filling of TPEE resin.

[0020] The oil-filled TPEE resin, 0.1-0.6 parts of antioxidant, 0.1-2 parts of lubricant and 0-3 parts of auxiliary agent are mixed and stirred, then melted, mixed and dispersed, 1-6 parts of pretreated polyester fibers are added, melt extruded and granulated to obtain a TPEE composite material.

[0021] After mixing 95-99.5wt% of TPEE composite material with 0.5-5 parts of chemical foaming agent masterbatch, the mixture is injection molded and foamed by a secondary mold opening process.

[0022] Preferably, the stirring time is 12 hours; and the heating temperature is 120°C.

[0023] Application of the above-mentioned TPEE foamed composite material or the composite material prepared by the above-mentioned preparation method in the preparation of automotive soft interior parts.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention greatly reduces the initial hardness and feel of TPEE materials on the market by directly performing high-temperature oil filling on TPEE resin, and introduces polyester fibers to form disordered network connections between TPEE foaming melts in the subsequent chemical injection molding mold opening and foaming process to avoid melt pulling and rupture during the mold opening process, so that it maintains continuous pores, and avoids the drawbacks of further reducing the melt strength of TPEE materials and deteriorating foaming performance caused by oil-filled plasticizers. The characteristics of low hardness, low melt strength but high foaming performance, and continuous closed non-collapsed pores are achieved, and a large-distance mold opening action can be performed to achieve high foaming product thickness and low surface hardness of good touch automotive soft interior materials. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] Take 2 parts of KH550 coupling agent and spray it evenly on the surface of 4 parts of polyester fiber to obtain pretreated polyester fiber, take 30 parts of cycloalkane oil plasticizer and 65 parts of 25D TPEE resin in a heating stirrer at 120°C and stir them for 12 hours to make TPEE fully swell and absorb to obtain oil-extended TPEE, then mix the oil-extended TPEE with 0.6 parts of antioxidant 1010, 2 parts of lubricant silicone masterbatch, 1 part of light stabilizer, 1 part of antistatic agent and 1 part of colorant, and then put them into a co-rotating twin-screw extruder for melting, mixing and dispersion, and put the pretreated polyester fiber into it through the side feeding port, and after melt extrusion and granulation, a TPEE composite material is obtained.

[0029] After 96 parts of the above TPEE composite material and 4 parts of the foaming agent masterbatch are uniformly mixed, a foamed TPEE composite material is obtained by injection molding and foaming using a secondary mold opening process.

[0030] Example 2

[0031] Take 3 parts of KH550 coupling agent and spray it evenly on the surface of 6 parts of polyester fiber to obtain pretreated polyester fiber, take 20 parts of cycloalkane oil plasticizer and 70 parts of 28D TPEE resin in a heating stirrer at 120°C and stir them for 12 hours to make TPEE fully swell and absorb to obtain oil-extended TPEE, then mix the oil-extended TPEE with 0.4 parts of antioxidant 1010, 0.1 parts of lubricant erucamide, 0.7 parts of light stabilizer, 0.5 parts of antistatic agent and 0.8 parts of colorant, and then put them into a co-rotating twin-screw extruder for melting, mixing and dispersion, and put the pretreated polyester fiber into it through the side feeding port, and after melt extrusion and granulation, a TPEE composite material is obtained.

[0032] After 97 parts of the above TPEE composite material and 3 parts of the foaming agent masterbatch are uniformly mixed, the mixture is injection molded by a secondary mold opening process to obtain a foamed TPEE composite material.

[0033] Example 3

[0034] 1.5 parts of KH560 coupling agent were sprayed uniformly on the surface of 3 parts of polyester fiber to obtain pretreated polyester fiber, 10 parts of cycloalkane oil plasticizer and 80 parts of 28D TPEE resin were fully stirred at 120°C in a heating stirrer for 12 hours to make TPEE fully swell and absorb to obtain oil-extended TPEE, and then the oil-extended TPEE was mixed with 0.1 parts of antioxidant 1010, 0.5 parts of lubricant polyethylene wax, 0.2 parts of ultraviolet absorber, 0.2 parts of antistatic agent and 0.1 parts of colorant, and then put into a co-rotating twin-screw extruder for melting, mixing and dispersion, and the pretreated polyester fiber was put in through the side feeding port, melt extruded and granulated to obtain a TPEE composite material.

[0035] 95 parts of the above TPEE composite material and 5 parts of the foaming agent masterbatch were uniformly mixed, and then injection molded by a secondary mold opening process to obtain a foamed TPEE composite material.

[0036] Example 4

[0037] Take 0.5 parts of KH550 coupling agent and spray it evenly on the surface of 1 part of polyester fiber to obtain pretreated polyester fiber, take 40 parts of cycloalkane oil plasticizer and 50 parts of 75D TPEE resin in a heating stirrer at 120°C and stir them for 12 hours to make TPEE fully swell and adsorb to obtain oil-filled TPEE, then mix the oil-filled TPEE with 0.3 parts of antioxidant 1010, 1 part of lubricant silicone masterbatch, 0.25 parts of ultraviolet absorber, 0.25 parts of antistatic agent and 0.5 parts of colorant, and then put them into a co-rotating twin-screw extruder for melting, mixing and dispersion, and put the pretreated polyester fiber into it through the side feeding port, and after melt extrusion and granulation, a TPEE composite material is obtained.

[0038] 99.5 parts of the above TPEE composite material and 0.5 parts of the foaming agent masterbatch were uniformly mixed, and then injection molded by a secondary mold opening process to obtain a foamed TPEE composite material.

[0039] Comparative Example 1

[0040] No pretreated polyester fiber was added, and other components, addition amounts and preparation methods were the same as those in Example 1.

[0041] Comparative Example 2

[0042] The TPEE resin is not oil-filled, and the corresponding oil-filling ratio is added to the TPEE resin. The other components, addition amounts and preparation methods are the same as those in Example 1.

[0043] Table 1: Performance of each sample in Examples 1 to 4 and Comparative Examples 1 to 2

[0044]

[0045] Pretreated polyester fibers are added to the TPEE composite materials in Example 1, Example 2, and Example 3. The experimental results show that the obtained composite materials have uniform and continuous pores. In Comparative Example 1, no pretreated polyester fibers are added, and the obtained composite materials have serious pore collapse. In addition, the TPEE composite materials in Example 1, Example 2, Example 3, and Example 4 are all oil-filled, and the obtained TPEE composite materials have a good hand feel, while Comparative Example 2 is not oil-filled, and the obtained composite material has a poor hand feel. Hot oil filling of TPEE resin can significantly reduce the hardness of TPEE material and improve the hand comfort, but further reduce the melt strength of TPEE, thereby reducing its foaming performance. The introduction of pretreated polyester fibers can compensate for the disadvantage of melt reduction, form disordered connections between TPEE foamed melts, ensure a larger mold opening distance and foaming thickness, and will not cause pore collapse. The low-hardness and good-touch TPEE foamed composite material prepared by the present invention has excellent foaming performance and excellent low-hardness and good touch, and has broad application prospects in automotive soft interior products.

[0046] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0047] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A TPEE foamed composite material, characterized in that: Including the following ingredients: TPEE resin 50-80 parts, plasticizer oil 10-40 parts, polyester fiber 1-6 parts, coupling agent 0.5-3 parts, antioxidant 0.1-0.6 parts, lubricant 0.1-2 parts, chemical foaming agent 0.5-5 parts and auxiliary agent 0-3 parts; The plasticizing oil includes one or more of paraffin oil, cycloparaffin oil, aromatic hydrocarbon oil and straight-chain paraffin oil; The polyester fibers are short-cut fibers.

2. The TPEE foamed composite material according to claim 1, characterized in that: The hardness of the TPEE resin is 25D-75D.

3. The TPEE foamed composite material according to claim 1, characterized in that: The chemical foaming agent includes one or more of NaHCO3 and azodicarbonamide.

4. The TPEE foamed composite material according to claim 1, characterized in that: The antioxidant includes one or more of hindered phenol, thioester and phosphite antioxidants.

5. The TPEE foamed composite material according to claim 1, characterized in that: The lubricant includes one or more of erucamide, calcium stearate, stearic acid amide, silicone masterbatch and polyethylene wax.

6. The TPEE foamed composite material according to claim 1, characterized in that: The coupling agent includes one or more of KH550 and KH560.

7. The TPEE foamed composite material according to claim 1, characterized in that: The auxiliary agent includes one or more of an ultraviolet light absorber, a light stabilizer, an antistatic agent and a colorant.

8. A method for preparing a TPEE foamed composite material, characterized in that: The following steps are involved: Spraying a coupling agent on the surface of the polyester fiber, wherein the mass ratio of the polyester fiber to the coupling agent is 2:1, to obtain a pretreated polyester fiber; Heat and mix 50-80 parts of TPEE resin and 10-40 parts of plasticizer oil, and stir to make TPEE swell and absorb the plasticizer oil until there is no plasticizer oil residue in the stirring pot and on the surface of TPEE resin, thus completing the oil filling of TPEE resin. The oil-filled TPEE resin, 0.1-0.6 parts of antioxidant, 0.1-2 parts of lubricant and 0-3 parts of auxiliary agent are mixed and stirred, then melted, mixed and dispersed, 1-6 parts of pretreated polyester fibers are added, melt extruded and granulated to obtain a TPEE composite material. After mixing 95-99.5wt% of TPEE composite material with 0.5-5 parts of chemical foaming agent masterbatch, the mixture is injection molded and foamed by a secondary mold opening process.

9. The method for preparing the TPEE foamed composite material according to claim 8, characterized in that: The stirring time is 12 hours; the heating temperature is 120°C.

10. Use of the TPEE foamed composite material according to any one of claims 1 to 7 or the composite material prepared by the preparation method according to claims 8 to 9 in the preparation of automotive soft interior parts.

Citation Information

Cited By

  • Low-temperature foaming thermoplastic polyester elastomer material as well as preparation method and application thereof

    CN121405912A