Microwave absorbent, wave-absorbing slurry, wave-absorbing patch and preparation method thereof
By mixing magnetic metal micropowder with microwave dielectric and magnetic dielectric materials in a specific proportion in the absorbent material, and combining resin matrix and air spraying technology, the problems of high density and low efficiency of traditional absorbent materials are solved, and light weight is achieved. Efficient wave absorption effect.
Patent Information
- Application Number
- CN202411033952.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Traditional wave absorbing materials have large body density, heavy mass, and low absorption efficiency, making them difficult to achieve ideal wave absorbing effects.
By mixing magnetic metal micropowder with microwave dielectric material and microwave magnetic dielectric material in a specific proportion, forming a composite absorber, and combining resin matrix to prepare absorbent slurry and patches, air spraying and rolling process are used to achieve uniform thickness and Highly efficient wave absorption.
It significantly reduces the density of the absorbing material, improves the absorption efficiency, and achieves wide-band and efficient electromagnetic wave absorption performance.
Smart Images

Figure CN118931244A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of absorbing materials, and in particular relates to a microwave absorber, a absorbing slurry, a absorbing patch and a preparation method thereof. Background Art
[0002] The confrontational development of radar stealth and detection technology and the popularization of various electronic devices have put forward urgent requirements for absorbing materials. High-performance microwave absorbing materials must have the characteristics of light weight, thin thickness, wide frequency band, and strong absorbing performance. In order to obtain high-performance absorbing coating materials, it is crucial to select reasonable absorbents, substrates and feasible processes. Resin, rubber and other matrix absorbing materials are widely used in the field of absorbing materials because of their simple preparation and molding process, flexibility and low production cost.
[0003] Developing high-performance absorbers is the key to improving the absorbing performance of absorbing coatings. Researching the electromagnetic properties, content and matching selection of absorbers is crucial to achieving ideal absorbing effects. Currently, absorbing materials on the market mostly rely on resin / rubber-based absorbing materials prepared by magnetic metal micropowders through specific processes. The main problems include high volume density and surface density, and excessive loss characteristics, resulting in a wide absorbing bandwidth but low absorbing efficiency, and thus single-phase absorbers are difficult to achieve ideal absorbing effects. The introduction of dual-loss absorbers can further optimize the absorbing performance of coatings by combining two different loss mechanisms. In particular, the preparation of lightweight dual-loss absorbers has extremely high practical significance for improving the comprehensive performance of absorbing materials. Summary of the invention
[0004] The purpose of the present invention is to provide a microwave absorber, an absorbing slurry, an absorbing patch and a preparation method thereof, which solve the problems of high bulk density, heavy mass and even low absorbing efficiency caused by the use of a large amount of magnetic metal micropowder as an absorber to prepare absorbing coatings in traditional absorbing materials.
[0005] The present invention is achieved through the following technical solutions:
[0006] A microwave absorber, comprising magnetic metal micropowder and microwave dielectric material;
[0007] The mass ratio of microwave dielectric material to magnetic metal powder is 1-7:1-3.
[0008] Furthermore, the magnetic metal powder is carbonyl iron powder or FeSiAl powder;
[0009] The microwave dielectric material is LiNb 0.8 Ti 0.25 O3 ceramic powder.
[0010] The invention also discloses a microwave absorbent, comprising magnetic metal micropowder and microwave magnetic medium material;
[0011] The mass ratio of microwave magnetic medium material to magnetic metal powder is 1 to 4:1.
[0012] Furthermore, the magnetic metal powder is carbonyl iron powder or FeSiAl powder;
[0013] The microwave magnetic medium material is ferrite material Ba3Co2Fe 24 O 41 of ceramic powder.
[0014] The invention also discloses a microwave absorbent, comprising magnetic metal micropowder, microwave dielectric material and microwave magnetic dielectric material;
[0015] The mass ratio of microwave dielectric material, microwave magnetic dielectric material and magnetic metal powder is (1-3):1:(1-3).
[0016] Furthermore, the magnetic metal powder is carbonyl iron powder or FeSiAl powder;
[0017] The microwave dielectric material is LiNb 0.8 Ti 0.25 O3 ceramic powder;
[0018] The microwave magnetic medium material is ferrite material Ba3Co2Fe 24 O 41 of ceramic powder.
[0019] The invention also discloses a preparation method of the microwave absorbent, which comprises mixing raw materials according to a designed ratio, ball milling, drying, grinding and sieving to obtain composite powder, thereby obtaining the microwave absorbent.
[0020] The present invention also discloses a microwave absorbing slurry, comprising a binder, a curing agent, a toughening agent, a defoaming agent, a dispersant and a solvent, and the microwave absorbent;
[0021] The binder, curing agent, toughening agent, defoaming agent, dispersant and microwave absorber are solidified materials. Taking the mass of the solidified materials as 100%, the total amount of the binder, curing agent, toughening agent, defoaming agent and dispersant accounts for 15% to 35%, and the microwave absorber accounts for 65% to 85%.
[0022] Further, the binder, curing agent, toughening agent, defoaming agent and dispersant are dissolved in acetone and mixed, and then uniformly dispersed to obtain a resin slurry;
[0023] The microwave absorber is added into the resin slurry and dispersed uniformly to obtain the microwave absorbing slurry.
[0024] The present invention also discloses a method for preparing an absorbing patch based on the absorbing slurry, comprising the following steps:
[0025] Cut the release paper into regular sizes and stick it on the metal substrate, and place it horizontally in the center of the water curtain cabinet;
[0026] Pour the absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times, adjust the airflow size and feed amount, and use air spraying to spray the absorbing slurry intermittently for multiple times, with the interval between each spraying being 3 to 8 minutes, to spray a coating with uniform thickness on the substrate;
[0027] After curing at room temperature, a semi-cured coating material is obtained, which is evenly torn off from the release paper to serve as a precursor of an absorbing patch;
[0028] In the semi-cured state, the absorbing patch precursor is rolled multiple times. According to the actual thickness of the patch, the thickness is reduced each time, and the rolling direction is continuously adjusted until the target thickness is reached.
[0029] After rolling, the metal plate is statically pressed and cured at room temperature to obtain the final absorbing patch.
[0030] Compared with the prior art, the present invention has the following beneficial technical effects:
[0031] The invention discloses a microwave absorber, comprising magnetic metal micropowder and microwave dielectric material; the microwave dielectric material is added to effectively adjust the real part of the microwave dielectric constant to adjust the impedance matching characteristics, thereby significantly enhancing the electromagnetic wave absorption effect. Compared with using only a single magnetic metal micropowder absorber, the coating and patch material prepared by the method of the invention have the advantages of low density and good absorption effect.
[0032] The invention discloses a microwave absorber, comprising magnetic metal micropowder and microwave magnetic medium material; the microwave magnetic medium material is added to effectively adjust the imaginary part of the magnetic permeability to adjust the impedance matching characteristics, thereby improving the electromagnetic wave absorption performance. Compared with the absorber using a high proportion of magnetic metal micropowder, the resin-based absorbing coating and patch material prepared by the method of the invention have the advantages of low volume density and surface density, high absorbing efficiency at a specific thickness, etc.
[0033] The present invention discloses a microwave absorber, including magnetic metal micropowder, microwave dielectric material and microwave magnetic dielectric material. The composite absorber has multiple losses such as dielectric loss, magnetic loss and conductivity loss, and has unique advantages in effectively and finely controlling the resistance and reactance of impedance matching. By adding dielectric materials, the capacitive reactance characteristics can be effectively improved, and by adding magnetic dielectric materials, the resistance characteristics can be effectively controlled, and the absorbing performance of the composite absorbing material can be synergistically optimized. Compared with the absorber using a high proportion of magnetic metal micropowder, the method of the present invention has the advantages of low volume density and surface density, high absorbing efficiency at a specific thickness, etc.
[0034] The invention discloses a method for preparing a microwave absorbing slurry, including the ratio of microwave absorbent to resin matrix, and the amount of toughening agent, defoaming agent and dispersant added to the microwave absorbing slurry. The total amount of binder, curing agent, toughening agent, defoaming agent and dispersant accounts for 15% to 35% of the total solid content of the microwave absorbing slurry by mass, and the microwave absorbent accounts for 65% to 85% of the total solid content of the microwave absorbing slurry by mass. The resin-based composite microwave absorbing slurry can be effectively regulated according to the absorbent ratio and thickness, and can meet the "thin, light, wide and strong" microwave absorbing effect of a specific frequency band according to actual needs.
[0035] The invention discloses a method for preparing an absorbing patch, wherein release paper is used as a contact layer when the patch is sprayed, so that the resin layer can be removed intact in a semi-cured state; in combination with the air spraying process, a dispersed absorbing slurry is poured into the feed chamber of the spray gun in small amounts and multiple times, the air flow size and the feed amount are adjusted, and the absorbing slurry is sprayed multiple times intermittently in a water curtain cabinet by an air spraying method, wherein the time interval between each spraying is 3 to 8 minutes, and a coating with uniform thickness is prepared on a substrate with release paper attached; when the coating is semi-cured, it is removed from the release paper for rolling, so as to realize the preparation of an absorbing patch with uniform thickness and flat surface, improve the smoothness and density of the patch, and strictly control the thickness of the absorbing patch. After the rolling is completed, it is placed at room temperature, and the absorbing patch is obtained after it is completely cured. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the preparation process of the present invention.
[0037] Figure 2 This is a physical picture of the absorbing patch prepared in Example 1.
[0038] Figure 3 The electromagnetic parameter diagrams of the absorbing patch prepared in Example 1: (a) shows the real part of the dielectric constant; (b) shows the imaginary part of the dielectric constant; (c) shows the real part of the magnetic permeability; (d) shows the imaginary part of the magnetic permeability.
[0039] Figure 4 The reflection loss diagram of the absorbing patch prepared in Example 1: (a) is a simulated reflection loss diagram at different thicknesses; (b) is a measured reflection loss diagram at a thickness of 1.6 mm.
[0040] Figure 5 The reflection loss diagram of the absorbing patch prepared in Example 2: (a) is a simulated reflection loss diagram at different thicknesses; (b) is a measured reflection loss diagram at a thickness of 1.7 mm.
[0041] Figure 6 This is the microscopic morphology of the composite powder prepared in Example 3.
[0042] Figure 7This is a cross-sectional microscopic morphology of the absorbing patch prepared in Example 3.
[0043] Figure 8 The reflection loss diagram of the absorbing patch prepared in Example 3: (a) is a simulated reflection loss diagram at different thicknesses; (b) is a measured reflection loss diagram at a thickness of 1.1 mm.
[0044] Fig. 9 The reflection loss diagram of the absorbing patch prepared in Example 4: (a) is a simulated reflection loss diagram at different thicknesses; (b) is a measured reflection loss diagram at a thickness of 1.3 mm. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments.
[0046] The components described and shown in the drawings and embodiments of the present invention may be arranged and designed in various configurations. Therefore, the detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of the claimed invention, but merely represents a selected embodiment of the present invention. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0047] It should be noted that the terms "comprises", "includes" or any other variations are intended to cover non-exclusive inclusion, so that a process, element, method, article or equipment that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to the process, element, method, article or equipment.
[0048] The invention discloses a microwave absorbent, which comprises magnetic metal micropowder, microwave dielectric material and / or microwave magnetic dielectric material to form a two-phase or three-phase composite.
[0049] Specifically, the microwave dielectric material is a microwave dielectric ceramic powder LiNb synthesized by a solid phase reaction method. 0.8 Ti 0.25 O3; the microwave magnetic medium material is a ferrite ceramic powder Ba3Co2Fe prepared by a solid phase reaction method 24 O 41; The magnetic metal micropowder is carbonyl iron powder or FeSiAl powder; the design of the lightweight absorber is universal for the selection of microwave dielectric materials with high dielectric constant, microwave magnetic dielectric materials with high magnetic permeability, and metal micropowders with high magnetic loss, so the protection scope of specific materials is not limited to the specific materials mentioned in the present invention.
[0050] The present invention also designs a microwave absorbing slurry, comprising a binder, a curing agent, a toughening agent, a defoaming agent, a dispersant and a solvent, and the microwave absorber; the binder, the curing agent, the toughening agent, the defoaming agent, the dispersant and the microwave absorber are solidified, and based on the mass of the solidified material being 100%, the total amount of the binder, the curing agent, the toughening agent, the defoaming agent and the dispersant accounts for 15% to 35%; the microwave absorber accounts for 65% to 85%.
[0051] The adhesive is bisphenol A epoxy resin E-40, the curing agent is polyamide 651, the toughening agent is water-based polyurethane P-522, and the solvent is acetone.
[0052] Bisphenol A epoxy resin has high transparency, strength and bonding strength, as well as certain toughness and corrosion resistance. E-40 epoxy resin is a relatively common resin. This type of resin can form a variety of cured products with excellent performance with a variety of curing agents, additives and absorbents. It basically does not produce small molecular volatiles during curing, has good processability and a simple preparation process. Polyamide 651 is a chemical substance used as a toughening curing agent for bisphenol epoxy resin, and its amine value is 380-450 mg / KOH / g. The curing conditions are room temperature curing for 48 hours or 65°C curing for 4 hours. The curing speed of polyamide 651 is faster than that of 650 low molecular weight polyamide. Therefore, the present invention uses bisphenol A type E-40 epoxy resin as a binder and polyamide 651 as a curing agent.
[0053] The present invention also discloses a method for preparing the microwave absorbent, which is specifically:
[0054] The magnetic metal powder, microwave dielectric material and / or microwave magnetic dielectric material are mixed, ball-milled for 10 to 20 hours, dried at 50° C., ground and sieved to obtain composite powder. Anhydrous ethanol is used as a grinding aid in the ball-milling process.
[0055] Also disclosed is a method for preparing an absorbing slurry, which comprises weighing specific amounts of epoxy resin, polyamide curing agent, water-based polyurethane, defoaming agent and dispersant, dispersing the mixture using a high-speed homogenizing disperser to obtain a resin slurry, then adding a composite powder to the resin slurry to obtain a composite slurry, and stirring and dispersing the composite slurry using a high-speed homogenizing disperser to obtain the absorbing slurry.
[0056] The microwave absorbing patch is prepared based on the microwave absorbing slurry obtained above, and the specific steps are as follows:
[0057] Cut the release paper into regular sizes and stick it on the metal substrate, then place it horizontally in the center of the water curtain cabinet;
[0058] Pour the absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times, adjust the appropriate air flow size and feed amount with the assistance of an air compressor, and use the air spray method to spray the composite slurry intermittently multiple times in a water curtain cabinet to prepare a coating with uniform thickness on a regular flat plate;
[0059] Spraying a sample of a specific thickness and size, and curing it at room temperature for 10 to 15 hours to obtain an epoxy resin-based lightweight absorbing coating composited with the dielectric, magnetic medium and magnetic metal micropowder, and peeling off the coating with a certain flexibility as a precursor of an absorbing patch;
[0060] In the semi-cured state, the absorbing patch is rolled multiple times using a rolling machine to improve the smoothness and density of the patch and control the thickness of the absorbing patch;
[0061] After rolling, the metal plate is statically pressed and cured at room temperature for 48 hours to obtain a finished lightweight absorbing patch.
[0062] The features and performances of the present invention are further described in detail below in conjunction with the embodiments.
[0063] Example 1
[0064] like Figure 1 As shown, the present embodiment prepares a method for preparing a lightweight magnetic medium material + magnetic metal powder composite resin-based absorbing patch, and the specific preparation method includes the following steps:
[0065] Step 1: Preparation of Ba3Co2Fe 24 O 41 (Co2Z) powder.
[0066] The raw materials BaCO3, Fe2O3, Co2O3 are Ba3Co2Fe 24 O 41 The raw materials were fully mixed by wet ball milling, and the mixed slurry after ball milling was completely dried at 50°C. After grinding and screening, the ferrite ceramic Ba3Co2Fe 24 O 41 Powder.
[0067] Step 2: Preparation of Co2Z@CIP composite powder.
[0068] Ba3Co2Fe 24 O 41The powder and granular CIP were weighed in a stainless steel ball mill at a mass ratio of 1:1, 2:1, 3:1, and 4:1, and then mixed with stainless steel balls with a diameter of 3 to 6 mm at a ball-to-material ratio of 10:1. Ba3Co2Fe 24 O 41 The powder and granular CIP powder were ball-milled for 18 hours. The Co2Z@CIP mixed slurry after ball milling was completely dried at 50°C, and four composite powders of magnetic medium material + magnetic metal powder with different mass ratios were obtained after grinding and sieving.
[0069] Step 3: Prepare resin slurry.
[0070] 20g of bisphenol A epoxy resin E-40 and 5g of curing agent polyamide 651 were dissolved in acetone, 3g of P-522 waterborne polyurethane, 1g of defoamer and 1g of dispersant were added, and then stirred and dispersed at a rate of 3kr / min for 10 minutes using a high-speed homogenizer to obtain a resin slurry.
[0071] Step 4: Prepare the microwave absorbing slurry.
[0072] Subsequently, 70 g of each of four Co2Z@CIP composite powders with different mass ratios were slowly poured into the above resin slurry, and then uniformly dispersed at a rate of 3 kr / min for 1 h using a high-speed homogenizer to obtain an absorbing slurry.
[0073] Step 5: Spray coating.
[0074] Pour the dispersed absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times. With the assistance of an air compressor, adjust the appropriate airflow size and feed amount. Use air spraying to spray the composite slurry intermittently in a water curtain cabinet for multiple times. The time interval between each spraying is 3 minutes, and a coating with uniform thickness is prepared on a regular flat plate.
[0075] Step 6: Rolling operation.
[0076] When the coating is semi-cured, it needs to be torn off the flat plate for rolling to reduce defects such as internal pores and cracks. By gradually reducing the thickness and changing the direction of rolling multiple times, the smoothness and density of the patch are improved, and the thickness of the absorbing patch is strictly controlled.
[0077] Step 7: Curing and forming.
[0078] After rolling, place it at room temperature and wait for it to completely solidify to obtain Figure 2 The Co2Z@CIP epoxy resin-based absorbing patch shown.
[0079] After testing the electromagnetic parameters of the Co2Z@CIP epoxy resin-based absorbing patch, the following results were obtained: Figure 3 The electromagnetic parameters shown, Figure 3 Figures (a) and (b) show that both the real and imaginary parts of the dielectric constant decrease as the proportion of the magnetic medium increases; Figure 3 Figures (c) and (d) in the figure show that by adding magnetic dielectric materials, the imaginary part of the magnetic permeability of the composite material can be significantly reduced while the real part of the magnetic permeability changes slightly. Since magnetic loss is the main loss mechanism of this type of material, the reduction of the real and imaginary parts of the dielectric constant will not significantly weaken the loss characteristics of the material. By effectively controlling the imaginary part of the magnetic permeability, the magnetic loss characteristics of the patch material can be controlled over a large range.
[0080] Table 1 shows the density of the patch materials with a mass ratio of 1:1, 2:1, 3:1, and 4:1, as well as the absorption bandwidth and absorption peak data at certain thicknesses. Among them, the patch materials with absorbers with a mass ratio of Co2Z to CIP of 1:1 and 2:1 have effective absorption bandwidths (RL≤-8dB) covering the X-band (8.2 to 12.4GHz) at thicknesses of 1.6mm and 1.9mm, respectively, and the densities are 2.08g / cm 3 and 1.96 g / cm 3 , the density of common absorbing patches on the market is greatly reduced. When the mass ratio of Co2Z to CIP is 3:1 and 4:1, the density of the patch material is slightly reduced, but the absorption peak and effective absorbing bandwidth in the X (8.2-12.4 GHz) and Ku (12.4-18 GHz) bands are weakened.
[0081] Table 1
[0082]
[0083] like Figure 4 As shown, the reflectivity test of the absorbing patch prepared in this embodiment is carried out, and the analysis and comparison are Figure 4 It can be seen from Figure (a) that the Co2Z@CIP patch prepared in this embodiment can meet the C2 full-band reflectivity of less than -8dB, the minimum reflection loss is -27dB (7.5GHz), and the effective absorption bandwidth is 4.87GHz (5.51~10.38GHz) at a thickness of 2.0mm when the composite absorber mass ratio is Co2Z:CIP=1:1. Figure 4 Figure (b) shows that the absorbing patch has a wide effective absorption bandwidth and good absorbing effect. By comparing the measured reflection loss with the simulated reflection loss, it can be found that the measured results are basically consistent with the simulation results.
[0084] Example 2
[0085] This embodiment provides a method for preparing a lightweight dielectric material + magnetic metal powder composite resin-based absorbing patch, and the specific preparation method includes the following steps:
[0086] Step 1: Prepare LNT powder.
[0087] First, according to LiNb 0.8 Ti 0.25 The raw materials Li2CO3, Nb2O5 and TiO2 were weighed separately in a dry environment with a stoichiometric ratio of O3. The raw materials were fully mixed by wet ball milling, and the mixed slurry after ball milling was completely dried at 50°C. After grinding and sieving, LNT powder was synthesized by solid phase reaction method.
[0088] Step 2: Prepare LNT@FeSiAl composite powder.
[0089] Weigh 100g of LNT and FeSiAl powders in a mass ratio of 2:3, 1:1 and 3:2 and put them into a stainless steel ball mill. Mix the composite powder with stainless steel balls with a diameter of 3-6mm at a ball-to-material ratio of 10:1. Use anhydrous ethanol as a grinding aid and use a planetary ball mill to mill LNT powder and FeSiAl powder for 18h at a speed of 250rpm. The LNT@FeSiAl mixed slurry after ball milling is completely dried, and four LNT@FeSiAl composite powders with different mass ratios are obtained after grinding and sieving.
[0090] Step 3: Prepare resin slurry.
[0091] Dissolve 20g of bisphenol A epoxy resin E-40 and 5g of polyamide 651 in acetone at a mass ratio of 4:1, add 3g of P-522 waterborne polyurethane, 1g of defoamer and 1g of dispersant, and then use a homogenizer to evenly disperse at a rate of 3kr / min for 10min.
[0092] Step 4: Prepare the microwave absorbing slurry.
[0093] Subsequently, 70 g of each of four LNT@FeSiAl composite powders with different mass ratios were slowly poured into the above resin slurry, and then uniformly dispersed at a rate of 3 kr / min for 1 h using a homogenizer to obtain an absorbing slurry.
[0094] Step 5: Spray coating.
[0095] Pour the dispersed absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times, adjust the appropriate airflow size and feed amount with the assistance of an air compressor, and use the air spray method to spray the composite slurry intermittently multiple times in a water curtain cabinet. The time interval between each spraying is 5 minutes, and a coating with uniform thickness is prepared on a regular flat plate.
[0096] Step 6: Rolling operation.
[0097] When the coating is semi-cured, it needs to be torn off the flat plate for rolling to reduce defects such as internal pores and cracks. By gradually reducing the thickness and changing the direction of rolling multiple times, the smoothness and density of the patch are improved, and the thickness of the absorbing patch is strictly controlled.
[0098] Step 7: Curing and forming.
[0099] After rolling, place it at room temperature for 48 hours, and after it is completely solidified, the Figure 2 The lightweight LNT@FeSiAl epoxy resin-based absorber patch shown.
[0100] like Figure 5 As shown, the reflectivity of the absorbing patch prepared in this embodiment is calculated and tested. Figure 5 It can be seen from Figure (a) that the LNT@FeSiAl patch prepared in this embodiment can meet the X-band reflectivity of less than -8dB at a thickness of 1.8mm when the composite absorber mass ratio is LNT:FeSiAl=2:3, the minimum reflection loss is -17.6dB (10.2GHz), and the effective absorption bandwidth is 4.3GHz (8.1~12.4GHz). Figure 5 From Figure (b), we can see that the absorbing patch has a wide effective absorption bandwidth and good absorbing effect, and the measured results are close to the simulation results.
[0101] Table 2 shows the density of the patch materials of 2:3, 1:1, and 3:2, as well as the absorption bandwidth and absorption peak data at certain thicknesses. Among them, when the mass ratio of LNT to FeSiAl is 2:3, the patch can achieve full coverage of the effective absorption bandwidth (RL≤-8dB) of the X-band (8.2~12.4GHz) at a thickness of 1.8mm, and the patch density is only 1.86g / cm 3 When the mass ratio of LNT to FeSiAl is 1:1, the patch can achieve full coverage of the effective absorption bandwidth (RL≤-8dB) of the C1 band (3.85~5.85GHz) at a thickness of 3.0mm, and the patch density is only 1.72g / cm 3 When the mass ratio of LNT to FeSiAl is 3:2, the effective absorption bandwidth of the patch at a thickness of 3 mm is weakened compared with the previous group, but the density is reduced.
[0102] Table 2
[0103]
[0104] Example 3
[0105] This embodiment provides a method for preparing a lightweight dielectric material + magnetic metal powder composite resin-based absorbing patch, and the specific preparation method includes the following steps:
[0106] Step 1: Prepare LNT powder.
[0107] First, according to LiNb 0.8 Ti 0.25 The raw materials Li2CO3, Nb2O5, and TiO2 were weighed separately in a dry environment with a stoichiometric ratio of O3. The raw materials were fully mixed by wet ball milling, and the LNT mixed slurry after ball milling was completely dried at 50°C. After grinding and sieving, the dielectric ceramic powder LiNb was synthesized by solid phase reaction method. 0.8 Ti 0.25 O3(LNT powder).
[0108] Step 2: Preparation of LNT@CIP composite powder.
[0109] 100 g of LNT powder and granular CIP were weighed and placed in a stainless steel ball mill at a mass ratio of 1:1, 2:1, 3:1 and 4:1, respectively. The composite powder was mixed with stainless steel balls with a diameter of 3 to 6 mm at a ball-to-material ratio of 10:1. Anhydrous ethanol was used as a grinding aid, and LNT powder and granular CIP powder were ball milled for 18 hours at a speed of 300 rpm in a planetary ball mill. The ball-milled LNT@CIP mixed slurry was completely dried, and four LNT@CIP composite powders with different mass ratios were obtained after grinding and sieving.
[0110] Step 3: Prepare resin slurry.
[0111] Dissolve 20g of bisphenol A epoxy resin E-40 and 5g of polyamide 651 in acetone, add 3g of toughening P-522 waterborne polyurethane, 1g of defoamer and 1g of dispersant, and then use a high-speed homogenizer to evenly disperse at a rate of 3kr / min for 10 minutes.
[0112] Step 4: Prepare the microwave absorbing slurry.
[0113] Subsequently, 70 g of four LNT@CIP composite powders with different mass ratios were respectively slowly poured into the above resin slurry, and then uniformly dispersed at a rate of 3 kr / min for 1 h using a high-speed homogenizer to obtain a composite slurry.
[0114] Step 5: Spray coating.
[0115] Pour the dispersed absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times. With the assistance of an air compressor, adjust the appropriate airflow size and feed amount. Use air spraying to spray the composite slurry intermittently in a water curtain cabinet multiple times. The time interval between each spraying is 6 minutes, and a coating with uniform thickness is prepared on a regular flat plate.
[0116] Step 6: Rolling operation.
[0117] When the coating is semi-cured, it needs to be torn off the flat plate for rolling to reduce defects such as internal pores and cracks. By gradually reducing the thickness and changing the direction of rolling multiple times, the smoothness and density of the patch are improved, and the thickness of the absorbing patch is strictly controlled.
[0118] Step 7: Curing and forming.
[0119] After rolling, the film was placed at room temperature for 48 hours, and after it was completely cured, the LNT@CIP epoxy resin-based absorbing patch was obtained.
[0120] After scanning electron microscopy observation of the composite powder, the following results were obtained: Figure 6 The SEM image shown clearly shows that a large number of LNT particles are coated on the flaky carbonyl iron powder, and some LNT particles are dispersed around the flaky carbonyl iron powder. Figure 7 From the SEM image shown, it can be clearly seen that part of the LNT particles are coated on the flaky carbonyl iron powder, and part of the LNT particles are dispersed around the carbonyl iron powder. It can also be seen that the absorbent LNT particles and the flaky CIP are relatively evenly dispersed in the resin matrix.
[0121] like Figure 8 As shown, the reflectivity of the absorbing patch prepared in this embodiment is tested and calculated. Figure 8 It can be seen from Figure (a) that the LNT@CIP patch prepared in this embodiment can meet the Ku full-band reflectivity of less than -8dB at a thickness of 1.1mm when the composite absorber mass ratio is LNT:CIP=1:1, the minimum reflection loss is -22.2dB (14.02GHz), and the effective absorption bandwidth is 7.34GHz (10.6~18GHz). Figure 8 Figure (b) shows that the absorbing patch has a wide effective absorption bandwidth and good absorbing effect. By comparing the measured reflection loss with the simulated reflection loss, it is shown that the measured results are close to the simulated results.
[0122] Table 3 shows the density of the patch materials at 1:1, 2:1, 3:1, and 4:1, as well as the absorption bandwidth and absorption peak data at certain thicknesses. When the mass ratio of LNT to CIP is 1:1 and 2:1 respectively, the effective absorption bandwidth of the patch material with a thickness of only 1.1 mm and 1.2 mm can cover the Ku band (12.4-18 GHz), and the density is only 1.93 g / cm 3 and 1.68 g / cm 3 When the mass ratio of LNT to CIP is 3:1, the effective absorption bandwidth of the patch material with a thickness of 1.7 mm can achieve full coverage of the X-band, and the density is 1.6 g / cm 3 When the mass ratio of LNT to CIP is 4:1, the effective absorption bandwidth of the patch with a thickness of 2.2 mm can achieve a high coverage of the C2 band (5.85-8.2 GHz), and the density is only 1.53 g / cm 3 .
[0123] Table 3
[0124]
[0125] Example 4
[0126] This embodiment provides a method for preparing a lightweight dielectric material + magnetic metal powder + magnetic dielectric material epoxy resin-based microwave absorbing coating, and the specific preparation method includes the following steps:
[0127] Step 1: Preparation of LNT powder by solid phase reaction method.
[0128] First, according to LiNb 0.8 Ti 0.25 The raw materials Li2CO3, Nb2O5 and TiO2 were weighed separately in a dry environment with a stoichiometric ratio of O3. The raw materials were fully mixed by wet ball milling, and the LNT mixed slurry after ball milling was completely dried at 50°C. After grinding and sieving, LNT powder was synthesized by solid phase reaction method.
[0129] Step 2: Prepare Co2Z powder.
[0130] The raw materials BaCO3, Fe2O3, Co2O3 are Ba3Co2Fe 24 O 41 The stoichiometric ratios were weighed in a dry environment. Several powder raw materials were mixed evenly by wet ball milling, and the Co2Z mixed slurry after ball milling was completely dried at 50°C. After grinding and sieving, Co2Z powder was synthesized by solid phase reaction method.
[0131] Step 3: Preparation of LNT@Co2Z@CIP composite powder.
[0132] 100 g of LNT, CIP and Co2Z powders were weighed in a stainless steel ball mill at a mass ratio of 1:1:1, 2:1:1 and 1:2:1, and the composite powders were mixed with stainless steel balls with a diameter of 3 to 6 mm at a ball-to-material ratio of 10:1. Anhydrous ethanol was used as the ball milling medium, and LNT, Co2Z powders and CIP powders were ball milled at a speed of 300 rpm in a planetary ball mill for 18 hours. The ball-milled LNT@Co2Z@CIP mixed slurry was completely dried, and three LNT@Co2Z@CIP composite powders with different mass ratios were obtained after grinding and sieving.
[0133] Step 4: Prepare resin slurry.
[0134] Dissolve 20g of bisphenol A epoxy resin E-40 and 5g of polyamide 651 in acetone, add 3g of P-522 waterborne polyurethane, 1g of defoamer and 1g of dispersant, and then use a high-speed homogenizer to evenly disperse at a rate of 3kr / min for 10 minutes.
[0135] Step 5: Prepare the microwave absorbing slurry.
[0136] Subsequently, 70 g of each of the three LNT@Co2Z@CIP composite powders with different mass ratios were slowly poured into the above resin slurry, and then uniformly dispersed at a rate of 3 kr / min for 1 hour using a high-speed homogenizer to obtain three different absorbing slurries.
[0137] Step 6: Spray coating.
[0138] Pour the dispersed absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times, adjust the appropriate airflow size and feed amount with the assistance of an air compressor, and use the air spray method to spray the composite slurry intermittently multiple times in a water curtain cabinet to prepare a coating with uniform thickness on a regular flat plate, with the time interval between each spraying being 8 minutes.
[0139] Step 7: Rolling operation.
[0140] When the coating is semi-cured, it needs to be torn off the flat plate for rolling to reduce defects such as internal pores and cracks. By gradually reducing the thickness and changing the direction of rolling multiple times, the smoothness and density of the patch are improved, and the thickness of the absorbing patch is strictly controlled.
[0141] Step 8: Curing and molding.
[0142] After rolling, it is placed at room temperature and completely cured to obtain a lightweight LNT@Co2Z@CIP epoxy resin-based absorbing patch.
[0143] like Fig. 9 As shown, the reflectivity of the absorbing patch prepared in this embodiment is tested and calculated. Fig. 9It can be seen from Figure (a) that the LNT@Co2Z@CIP patch prepared in this embodiment can meet the Ku full-band reflectivity of less than -8dB at a thickness of 1.3mm when the composite absorber mass ratio is LNT:Co2Z:CIP=2:1:1, the minimum reflection loss is -29.3dB (15.3GHz), and the effective absorption bandwidth is 5.1GHz (12.4~17.5GHz). By observing and comparing Fig. 9 Figure (b) shows that the absorbing patch has a wide effective absorption bandwidth and good absorbing effect. By comparing the measured reflection loss with the simulated reflection loss, it can be found that the measured results are basically consistent with the simulation results.
[0144] Table 4 shows the density of patch materials with mass ratios of LNT, Co2Z and CIP of 1:1:1, 2:1:1 and 1:1:2, as well as the absorption bandwidth and absorption peak data at certain thicknesses. At a thickness of 1.4 mm, they can achieve effective absorption bandwidths of 5.2 GHz, 5.9 GHz and 5 GHz in the range of 2 to 18 GHz, respectively, with the strongest absorption peaks of -22.5 dB, -21.5 dB and -34.4 dB, respectively, and the density does not exceed 1.9 g / cm 3 , is a dual-band broadband absorbing material with great potential.
[0145] Table 4
[0146]
[0147] The present invention provides a design and preparation method of an epoxy resin-based lightweight absorbing material composited with microwave dielectric material or / and microwave magnetic dielectric material and magnetic metal micropowder. By adding an appropriate amount of microwave dielectric material and microwave magnetic dielectric material ceramic powder to the magnetic metal micropowder, the electromagnetic parameters can be effectively adjusted to achieve impedance matching and good attenuation characteristics, thereby obtaining a good absorbing effect. In addition, the density of the dielectric and magnetic dielectric ceramic powders with a relatively light weight is much lower than that of the metal powder, so the volume density and surface density of the absorbing slurry can be greatly reduced. At the same time, the present invention has the characteristics of simple preparation process, good plasticity and toughness, light weight, excellent electromagnetic properties and absorbing properties.
[0148] The present invention mainly adjusts the ratio of microwave dielectric material, microwave magnetic dielectric material and magnetic metal powder in the composite absorber to adjust the high-frequency resistance and reactance characteristics of the patch within a large range and effectively achieve impedance matching. That is, by compounding microwave dielectric material, microwave magnetic dielectric material and magnetic metal powder in two phases and three phases, optimizing the ratio of different types of absorbers, and coupling the multiple loss mechanisms of electric dipole, magnetic dipole and hysteresis current in the microwave electromagnetic field, optimizing the impedance matching characteristics in a specific frequency band, improving the absorbing performance of the composite coating and broadening the absorption band, thereby providing a relevant basis for the subsequent research and development of absorbing coatings.
[0149] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A microwave absorbent, characterized in that: Including magnetic metal powder and microwave dielectric materials; The mass ratio of microwave dielectric material to magnetic metal powder is 1-7:1-3.
2. A microwave absorbent according to claim 1, characterized in that: The magnetic metal powder is carbonyl iron powder or FeSiAl powder; The microwave dielectric material is LiNb 0.8 Ti 0.25 O3 ceramic powder.
3. A microwave absorbent, characterized in that: Including magnetic metal powder and microwave magnetic medium materials; The mass ratio of microwave magnetic medium material to magnetic metal powder is 1 to 4:
1.
4. A microwave absorbent according to claim 3, characterized in that: The magnetic metal powder is carbonyl iron powder or FeSiAl powder; The microwave magnetic medium material is ferrite material Ba3Co2Fe 24 O 41 of ceramic powder.
5. A microwave absorbent, characterized in that: Including magnetic metal powder, microwave dielectric material and microwave magnetic dielectric material; The mass ratio of microwave dielectric material, microwave magnetic dielectric material and magnetic metal powder is (1-3):1:(1-3).
6. A microwave absorbent according to claim 5, characterized in that: The magnetic metal powder is carbonyl iron powder or FeSiAl powder; The microwave dielectric material is LiNb 0.8 Ti 0.25 O3 ceramic powder; The microwave magnetic medium material is ferrite material Ba3Co2Fe 24 O 41 of ceramic powder.
7. The method for preparing the microwave absorbent according to any one of claims 1 to 6, characterized in that: The raw materials are mixed according to the designed proportions, ball-milled, dried, ground and sieved to obtain composite powder, thereby obtaining the microwave absorbent.
8. A microwave absorbing slurry, characterized in that: It comprises a binder, a curing agent, a toughening agent, a defoaming agent, a dispersant and a solvent, and the microwave absorber according to any one of claims 1 to 6; The binder, curing agent, toughening agent, defoaming agent, dispersant and microwave absorber are solidified materials. Taking the mass of the solidified materials as 100%, the total amount of the binder, curing agent, toughening agent, defoaming agent and dispersant accounts for 15% to 35%, and the microwave absorber accounts for 65% to 85%.
9. The method for preparing the microwave absorbing slurry according to claim 8, characterized in that: The binder, curing agent, toughening agent, defoaming agent and dispersant are dissolved in acetone, mixed and uniformly dispersed to obtain a resin slurry; The microwave absorber is added into the resin slurry and dispersed uniformly to obtain the microwave absorbing slurry.
10. A method for preparing an absorbing patch based on the absorbing slurry according to claim 8, characterized in that: The following steps are involved: Cut the release paper into regular sizes and stick it on the metal substrate, and place it horizontally in the center of the water curtain cabinet; Pour the absorbing slurry into the feed chamber of the spray gun in small amounts and multiple times, adjust the airflow size and feed amount, and use air spraying to spray the absorbing slurry intermittently for multiple times, with the interval between each spraying being 3 to 8 minutes, to spray a coating with uniform thickness on the substrate; After curing at room temperature, a semi-cured coating material is obtained, which is evenly torn off from the release paper to serve as a precursor of an absorbing patch; In the semi-cured state, the absorbing patch precursor is rolled multiple times. According to the actual thickness of the patch, the thickness is reduced each time, and the rolling direction is continuously adjusted until the target thickness is reached. After rolling, the metal plate is statically pressed and cured at room temperature to obtain the final absorbing patch.
Citation Information
Patent Citations
Textured lithium-niobium-titanium (Li-Nb-Ti-O) microwave medium ceramic and preparation method thereof
CN102211932A
Dielectric porcelain composition
JP1997110522A
Cited By
Temperature-resistant resin-based magnetoelectric composite wave-absorbing coating as well as preparation method and application thereof