Super-wear-resistant transparent super-hydrophobic coating and preparation method thereof
Through the combination of hydroxy fluororesin, amino silicone oil and modified silica nanoparticles, a stable system is formed using resonant acoustic mixing technology, which solves the problems of cumbersome coating preparation, poor wear resistance and insufficient transparency in the prior art. It realizes simple and efficient superhydrophobic coating preparation, suitable for large-scale applications and improves the wear resistance and transparency of the coating.
Patent Information
- Application Number
- CN202411062508.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ultra-wear-resistant transparent superhydrophobic coating is cumbersome in the preparation process and is not suitable for large-scale applications. It has poor wear resistance and insufficient transparency, which limits its application in the field of high optical demand.
Using a combination of hydroxy fluororesin, amino silicone oil, modified silica nanoparticles and environmentally friendly diluents, a stable system is formed through resonant acoustic mixing technology, and covalently grafted with the resin matrix using amino functionalized modified silica nanoparticles. , the chain segments of silicone oil and fluororesin are combined to reduce surface tension, and the coating is prepared by spraying to form a microstructure less than 100 nm to improve wear resistance and transparency.
It realizes simple superhydrophobic coating preparation, is suitable for large-scale applications, significantly improves the wear resistance and transparency of the coating, takes into account superhydrophobicity and transparency, and is suitable for areas with high optical demand.
Smart Images

Figure CN118931267A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a coating and a preparation method thereof, and specifically to a super wear-resistant transparent super hydrophobic coating and a preparation method thereof. Background Art
[0002] Super wear-resistant transparent super hydrophobic coatings have great potential application value in applications with high optical requirements, such as automobile windshields, building window glass, swimming goggles and eyepieces. However, on the one hand, the coating surface must have a high roughness to obtain a high contact angle. And the increase in roughness will reduce transparency due to light scattering. In order to take into account both transparency and super hydrophobicity, it is necessary to select a suitable roughness (less than 100nm). On the other hand, the wear resistance of transparent coatings has always been a challenge in the coatings industry. If the coating is worn, the transparent coating will be damaged, at least from an aesthetic point of view. Therefore, the coatings industry has been looking for ways to improve the wear resistance and transparency of super hydrophobic coatings.
[0003] Chinese patent CN107022279A discloses a method for preparing a super-hydrophobic coating having both transparency and good mechanical properties, the method adopts an organic-inorganic hybrid method to prepare a super-hydrophobic coating, and finally the coating is applied to the substrate by a scraping method, and the scraping method is not suitable for large-scale and complex-shaped substrates, so it is not suitable for large-scale applications. Chinese patent CN108101385A discloses a small-sized, uniformly distributed polymethyl methacrylate / silicon dioxide core / shell microparticle composite microsphere, and fluorination treatment is performed on it, and finally a high light transmittance, high contact angle coating is obtained with PDMS as an interlayer. However, the wear resistance of the coating is not good. Chinese patent CN106517821A discloses a kind of PDMS as a silicon source, multi-walled carbon nanotubes as a template, and a silicon nanotube coating is constructed on a glass surface, and then the PDMS solidified by chemical vapor deposition is hydrophobized to it, and finally a super wear-resistant transparent super-hydrophobic coating is obtained. However, the coating preparation is cumbersome and not suitable for large-scale applications.
[0004] The Chinese patent with publication number CN114854311A discloses a super-hydrophobic coating prepared on a concrete base surface by a construction method of spraying, brushing or rolling. However, the coating described in the patent is insufficient in transparency, which limits its application in areas with high optical requirements. In general, the existing super-hydrophobic coating has the problems of cumbersome preparation, unsuitable for large-scale application, poor wear resistance and poor transparency. Summary of the invention
[0005] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a super wear-resistant transparent super hydrophobic coating that is simple, convenient and suitable for large-scale production. Another purpose of the present invention is to provide a super wear-resistant transparent super hydrophobic coating.
[0006] Technical solution: The method for preparing a super wear-resistant transparent super hydrophobic coating according to the present invention comprises the following steps:
[0007] Step 1, mixing hydroxy fluororesin, amino silicone oil, modified silica nanoparticles 1, modified silica nanoparticles 2, a wetting dispersant and an environmentally friendly diluent to obtain a modified fluororesin, wherein the particle size of silica in the modified silica nanoparticles 1 is 10 to 20 nm, and the particle size of silica in the modified silica nanoparticles 2 is 50 to 100 nm;
[0008] Step 2, mixing a curing agent, an environmentally friendly diluent, a leveling agent, and a defoaming agent to obtain an active hydrogen-containing resin;
[0009] Step 3, resonantly mixing the modified fluororesin and the active hydrogen-containing resin to obtain a mixed solution;
[0010] Step 4: spray the mixed solution onto the base surface to obtain an ultra-wear-resistant, transparent, and ultra-hydrophobic coating.
[0011] Furthermore, in step 1, the mass ratio of hydroxy fluororesin, amino silicone oil, modified silica nanoparticles 1, modified silica nanoparticles 2, wetting dispersant, and environmentally friendly diluent is 54:10-12:5:1-3:1-3:25.5-29. The preparation methods of modified silica nanoparticles 1 and modified silica nanoparticles 2 are the same. The preparation method of modified silica nanoparticles 1 is: after ultrasonically dispersing silica and acetone, γ-aminopropylmethyldimethoxysilane is added, and the mass ratio of γ-aminopropylmethyldimethoxysilane to silica is 1:1-1:5, electromagnetic stirring is performed, centrifugation is performed, and solid precipitates are collected, and finally washed and dried with acetone.
[0012] Further, in step 1, the hydroxy fluororesin is any one of GK570, JF-2X, and JF-3X, the amino silicone oil is any one of HY-2300, OFX-8040A, and OFX-8209A, the wetting and dispersing agent is any one of BYK-111, BYK-163, BYK-220s, and BYK-P104s, and the environmentally friendly diluent is any one of propyl carbonate, dimethyl succinate, and butyl carbonate. The stirring speed is 2000 to 2200 r / min, and the time is 10 to 15 min. Preferably, the stirring speed is 2000 r / min, and the time is 10 min.
[0013] Furthermore, in step 2, the mass ratio of the curing agent, the environmentally friendly diluent, the leveling agent and the defoaming agent is 6-10:9-13:0.5:0.5.
[0014] Furthermore, in step 2, the curing agent is any one of HDI, N3390, and HDI trimer, the environmentally friendly diluent is any one of propylene carbonate, dimethyl butanedicarboxylate, and butyl carbonate, the leveling agent is any one of BYK300, BYK306, and BYK333, and the defoaming agent is any one of AF-8014, BYK-085, and BYK-088.
[0015] Furthermore, in step three, the mixed solution is a monodisperse mixture, and the particle size is less than 100 nm.
[0016] Furthermore, in step four, the spraying air pressure is 0.5-0.6 MPa, the distance between the spray gun and the base surface is 15-20 cm, and the spraying time is 10-15 s.
[0017] The super-wear-resistant, transparent and super-hydrophobic coating obtained by the preparation method of the super-wear-resistant, transparent and super-hydrophobic coating has a light transmittance of 89.5-93.5%.
[0018] Preparation principle: two kinds of silica nanoparticles with a particle size less than 100nm are selected, and they are modified by YDH-660 to form amino-functionalized modified silica nanoparticles, and then the two modified silica nanoparticles and amino silicone oil are covalently grafted to the resin matrix by the chemical reaction of amino group and curing agent polyisocyanate to form a stable system, so as to achieve the effect of improving the wear resistance of the coating; a microstructure is formed by assembling the two silica nanoparticles, and the polysiloxane segments in the silicone oil and the carbon fluorine segments in the fluororesin are used to reduce the surface tension, giving the coating super-hydrophobicity; in addition, the coating mixture is dispersed by resonant acoustic mixing technology to solve the agglomeration problem between the modified silica nanoparticles, so that the coating surface forms a microstructure less than 100nm, giving the coating transparency. In the present invention, the synergistic effect of multiple components can make the coating have super-hydrophobic, wear-resistant and transparent effects.
[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0020] 1. The obtained super-hydrophobic coating is easy to prepare, suitable for large-scale applications, and has good wear resistance;
[0021] 2. While introducing amino silicone oil and fluororesin to reduce the surface tension of the coating, two modified silica nanoparticles with different particle sizes are used to form a roughness of less than 100nm on the coating surface, so as to take into account the super hydrophobicity and transparency of the coating;
[0022] 3. Both modified silica nanoparticles and amino silicone oil are covalently linked to the resin matrix, which greatly improves the wear resistance of the superhydrophobic coating and solves the agglomeration problem of silica nanoparticles through resonant acoustic mixing technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a microstructure diagram of the coating of Example 2 of the present invention;
[0024] Figure 2 is a graph showing the wear resistance variation trend of the coating in Example 2 of the present invention;
[0025] Figure 3 This is a microstructure diagram of the coating of Comparative Example 2-1;
[0026] Figure 4 This is a graph showing the wear resistance variation trend of the coating of Comparative Example 2-1;
[0027] Figure 5 This is a microstructure diagram of the coating of Comparative Example 2-2;
[0028] Figure 6 This is a graph showing the wear resistance variation trend of the coating of Comparative Example 2-2. DETAILED DESCRIPTION
[0029] In the following examples, the raw materials and reagents are all industrial grade and commercially available. The manufacturers and models of the raw materials are as follows:
[0030] 1. Silica nanoparticles①
[0031] (1) Model 999121, Beijing Bailingwei Technology Co., Ltd., particle size ~20 nm;
[0032] (2) Model 134256, Chengdu Aikoda Chemical Reagent Co., Ltd., particle size ~15 nm.
[0033] 2. Silica Nanoparticles②
[0034] (1) Model 952360, Beijing Bailingwei Technology Co., Ltd., particle size ~50 nm;
[0035] (2) Model 989213, Beijing Bailingwei Technology Co., Ltd., particle size ~90 nm.
[0036] 3. Silica micro-nanoparticles
[0037] Model S5505, Beijing Bailingwei Technology Co., Ltd., particle size 0.2-0.3μm.
[0038] 4. Hydroxyfluororesin
[0039] (1) GK570, Daikin Fluorochemical (China) Co., Ltd., hydroxyl value 60±5 mgKOH / g;
[0040] (2) JF-2X, Sanaifu Zhonghao Chemical New Materials Co., Ltd., hydroxyl value 50±5 mgKOH / g;
[0041] (3) JF-3X, San Ai Fu Zhong Hao Chemical New Materials Co., Ltd., hydroxyl value 50 ± 5 mgKOH / g.
[0042] 5. Amino silicone oil
[0043] (1) HY-2300, Shanghai Huiyan New Materials Co., Ltd., viscosity 60-150cp, 25℃;
[0044] (2) OFX-8040A, Dow Chemical, viscosity 800-5000cp, 25°C;
[0045] (3) OFX-8209A, Dow Chemical, viscosity 300-1200 cp, 25°C.
[0046] 6. Aliphatic isocyanate curing agent
[0047] (1) HDI, produced by BASF (China) Co., Ltd., industrial product name Basonat HB 175MP / X CN, NCO content of 16-17%;
[0048] (2) N3390, produced by Bayer (China) Co., Ltd., industrial product name N3390, NCO content is (19.6±0.3)%;
[0049] (3) HDI trimer, produced by BASF (China) Co., Ltd., industrial product name Basonat HI 100ap, NCO content is 21.5% to 22.5%.
[0050] 7. Wetting and dispersing agent:
[0051] (1) BYK-163 (hereinafter referred to as “BYK-163”);
[0052] (2) BYK-P104s (hereinafter referred to as “BYK-P104s”);
[0053] (3) Produced by BYK Chemicals, model number BYK-111 (hereinafter referred to as “BYK-111”).
[0054] 8. Environmentally friendly diluent:
[0055] (1) Propyl carbonate, produced by Bailingwei Technology Co., Ltd., industrial grade;
[0056] (2) Dimethyl butanedicarboxylate, produced by Bailingwei Technology Co., Ltd., industrial grade;
[0057] (3) Butyl carbonate, produced by Bailingwei Technology Co., Ltd., industrial grade.
[0058] 9. Leveling agent:
[0059] (1) BYK-306 (hereinafter referred to as “BYK-495”) produced by BYK Chemical Company;
[0060] (2) BYK-333 manufactured by BYK Chemicals (hereinafter referred to as “BYK-333”);
[0061] (2) Produced by BYK Chemicals, model number BYK-300 (hereinafter referred to as “BYK-300”).
[0062] 10. Defoaming agent:
[0063] (1) Model AF-8014 manufactured by The Dow Chemical Company (hereinafter referred to as “AF-8014”);
[0064] (2) BYK-088 (hereinafter referred to as “BYK-088”);
[0065] (3) Produced by BYK Chemicals, model number BYK-085 (hereinafter referred to as “BYK-085”).
[0066] Example 1
[0067] A method for preparing a super wear-resistant transparent super hydrophobic coating comprises the following steps:
[0068] (1) 3 g of silica nanoparticles ① (model 999121, particle size ~20 nm) / silicon dioxide nanoparticles ② (model 989213, particle size ~90 nm) and acetone (100 mL) were added to a 250 mL round-bottom flask and ultrasonically dispersed for 30 min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1 g) was added to the reaction flask, and after electromagnetic stirring for 2 h, the mixture was centrifuged (2000 r / min, 10 min) and the solid precipitate was collected. Finally, the mixture was washed and dried with acetone to obtain modified silica nanoparticles ① (modified silica nanoparticles 1) and modified silica nanoparticles ② (modified silica nanoparticles 2).
[0069] (2) With the mechanical disperser agitator turned on at 1000 r / min, 29 g of environmentally friendly diluent propylene carbonate, 54 g of hydroxy fluororesin GK570, 1 g of wetting dispersant BYK-163, 5 g of modified silica nanoparticles ①, 1 g of modified silica nanoparticles ② and 10 g of amino silicone oil HY-2300 were added in sequence, and stirring was continued for 30 min to obtain component A modified fluororesin.
[0070] (3) 10 g of curing agent HDI, 9 g of environmentally friendly diluent propylene carbonate, 0.5 g of leveling agent BYK-306, and 0.5 g of defoaming agent AF-8014 were added to a beaker in sequence, and stirred at 2000 r / min for 10 min at room temperature to obtain a B component curing system (containing active hydrogen resin).
[0071] (4) Component A and component B were placed in a resonant acoustic mixing device at a mass ratio of 5:1, and treated for 15 minutes at a frequency of 80 Hz and an amplitude of 1.0 mm to obtain a mixed solution.
[0072] (5) Spray the mixed solution onto the treated glass substrate, with a coating thickness of 1.5 mm, a single-pass coating thickness of 1 mm, and two passes. The spraying process conditions are: air pressure 0.6 MPa, a distance of 20 cm between the spray gun and the substrate, a spraying time of 10 s, and uniform coating to obtain an ultra-wear-resistant, transparent, and ultra-hydrophobic coating.
[0073] Comparative Example 1-1
[0074] A method for preparing a super-hydrophobic coating comprises the following steps:
[0075] Under the condition that the mechanical dispersing stirrer is turned on at 1000r / min, 29g of environmentally friendly diluent propylene carbonate, 54g of hydroxy fluororesin GK570, 1g of wetting dispersant BYK-163, 5g of unmodified silica nanoparticles ① (model 999121), 1g of unmodified silica nanoparticles ② (model 989213) and 10g of amino silicone oil HY-2300 are added in sequence, and stirring is continued for 30min to obtain component A modified fluororesin; 10g of curing agent HDI, 9g of environmentally friendly diluent propylene carbonate, 0.5g of leveling agent BYK-306, and 0.5g of defoaming agent AF-8014 are added in sequence to a beaker, and stirred at 2000r / min for 10min at room temperature to obtain component B curing system; component A and component B are placed in a resonant acoustic mixing device at a mass ratio of 4:1, and treated for 15min at a frequency of 80Hz and an amplitude of 1.0mm to obtain a mixed solution. The mixed liquid was sprayed onto the same base surface as in Example 1 according to the same process parameters as in Example 1 to obtain a coating.
[0076] Comparative Example 1-2
[0077] A method for preparing a super-hydrophobic coating comprises the following steps:
[0078] 3g of silica nanoparticles ① (model 999121) / silica microparticles (model S5505) and acetone (100mL) were added to a 250mL round-bottom flask and ultrasonically dispersed for 30min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1g) was added to the reaction bottle, and after electromagnetic stirring for 2h, the solid precipitate was centrifuged (2000r / min, 10min) and collected. Finally, the modified silica nanoparticles ① and modified silica microparticles were obtained by washing and drying with acetone.
[0079] Under the condition of opening the mechanical dispersing stirrer at 1000r / min, 29g of environmentally friendly diluent propylene carbonate, 54g of hydroxyl fluororesin GK570, 1g of wetting dispersant BYK-163, 5g of modified silica nanoparticles①, 1g of modified silica microparticles and 10g of amino silicone oil HY-2300 were added in sequence, and stirring was continued for 30min to obtain component A modified fluororesin; 10g of curing agent HDI, 9g of environmentally friendly diluent propylene carbonate, 0.5g of leveling agent BYK-306, and 0.5g of defoaming agent AF-8014 were added in sequence in a beaker, and stirred at 2000r / min for 10min at room temperature to obtain component B curing system; component A and component B were placed in a resonant acoustic mixing device at a mass ratio of 4:1, and treated for 15min at a frequency of 80Hz and an amplitude of 1.0mm to obtain a mixed solution. The mixed solution was sprayed on the base surface of embodiment 1 according to the same process parameters as embodiment 1 to obtain a coating.
[0080] Example 2
[0081] A method for preparing a super wear-resistant transparent super hydrophobic coating comprises the following steps:
[0082] (1) 3 g of silica nanoparticles ① (model 134256, particle size ~15 nm) / silica nanoparticles ② (model 952360, ~50 nm) and acetone (100 mL) were added to a 250 mL round-bottom flask and ultrasonically dispersed for 30 min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1 g) was added to the reaction flask, and after electromagnetic stirring for 2 h, the solid precipitate was centrifuged (2000 r / min, 10 min) and collected. Finally, the modified silica nanoparticles ① and ② were obtained by washing and drying with acetone.
[0083] (2) With the mechanical dispersing stirrer turned on at 1000 r / min, 25.5 g of environmentally friendly diluent dimethyl butanedicarboxylate, 54 g of hydroxy fluororesin JF-2X, 1 g of wetting dispersant BYK-P104s, 5 g of modified silica nanoparticles ①, 2.5 g of modified silica nanoparticles ② and 12 g of amino silicone oil OFX-8040A were added in sequence, and stirring was continued for 30 min to obtain component A modified fluororesin.
[0084] (3) Add 6.5 g curing agent N3390, 12.5 g environmentally friendly diluent dimethyl succinate, 0.5 g leveling agent BYK-333, and 0.5 g defoaming agent BYK-088 into a beaker, and stir at 2000 r / min for 10 min at room temperature to obtain the B component curing system.
[0085] (4) Component A and component B were placed in a resonant acoustic mixing device at a mass ratio of 5:1, and treated for 20 minutes at a frequency of 120 Hz and an amplitude of 2.0 mm to obtain a mixed solution.
[0086] (5) Spray the mixed solution onto the treated glass substrate, with a coating thickness of 3.0 mm, a single-pass coating thickness of 0.5 mm, and two passes. The spraying process conditions are: air pressure 0.6 MPa, a distance of 20 cm between the spray gun and the substrate, a spraying time of 10 s, and uniform coating to obtain a super-wear-resistant and super-hydrophobic coating.
[0087] Comparative Example 2-1
[0088] A method for preparing a super-hydrophobic coating comprises the following steps:
[0089] 25.5 g of environmentally friendly diluent dimethyl butanedicarboxylate, 54 g of hydroxy fluororesin JF-2X, 1 g of dispersant BYK-P104s, 5 g of unmodified silica nanoparticles ① (model 134256), 2.5 g of unmodified silica nanoparticles ② (model 952360) and 12 g of amino silicone oil OFX-8040A were added in sequence under the condition of a mechanical dispersing stirrer at 1000 r / min, and stirring was continued for 30 min to obtain component A modified fluororesin grease; add 6.5g curing agent N3390, 12.5g environmentally friendly diluent dimethyl succinate, 0.5g leveling agent BYK-333, and 0.5g defoaming agent BYK-088 in a beaker, stir at 2000r / min for 10min at room temperature to obtain a B component curing system; put component A and component B into a resonant acoustic mixing device at a mass ratio of 5:1, and treat for 20min at a frequency of 120Hz and an amplitude of 2.0mm to obtain a mixed solution. Spray the mixed solution on the same base surface as in Example 2 according to the same process parameters as in Example 2 to obtain a coating.
[0090] Comparative Example 2-2
[0091] A method for preparing a super-hydrophobic coating comprises the following steps:
[0092] 3g of silica nanoparticles ① (model 134256) / silica microparticles (model S5505) and acetone (100mL) were added to a 250mL round-bottom flask and ultrasonically dispersed for 30min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1g) was added to the reaction bottle, and after electromagnetic stirring for 2h, the solid precipitate was centrifuged (2000r / min, 10min) and collected. Finally, the modified silica nanoparticles ① and modified silica microparticles were obtained by washing and drying with acetone.
[0093] Under the condition that the mechanical dispersing stirrer is turned on at 1000r / min, 25.5g of environmentally friendly diluent dimethyl butanedicarboxylate, 54g of hydroxy fluororesin JF-2X, 1g of dispersant BYK-P104s, 5g of modified silica nanoparticles①, 2.5g of modified silica microparticles and 12g of amino silicone oil OFX-8040A are added in sequence, and stirring is continued for 30min to obtain component A modified fluororesin; 6.5g of curing agent N3390, 12.5g of environmentally friendly diluent dimethyl butanedicarboxylate, 0.5g of leveling agent BYK-333 and 0.5g of defoaming agent BYK-088 are added in sequence in a beaker, and stirred at 2000r / min for 10min at room temperature to obtain component B curing system; component A and component B are placed in a resonant acoustic mixing device at a mass ratio of 5:1, and treated for 20min at a frequency of 120Hz and an amplitude of 2.0mm to obtain a mixed solution. The mixed liquid was sprayed onto the same base surface as in Example 2 according to the same process parameters as in Example 2 to obtain a coating.
[0094] Example 3
[0095] A method for preparing a super wear-resistant transparent super hydrophobic coating comprises the following steps:
[0096] (1) 3 g of silica nanoparticles ① (model 999121, particle size ~20 nm) / silicon dioxide nanoparticles ② (model 989213, particle size ~90 nm) and acetone (100 mL) were added to a 250 mL round-bottom flask and ultrasonically dispersed for 30 min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1 g) was added to the reaction flask, and after electromagnetic stirring for 2 h, the solid precipitate was centrifuged (2000 r / min, 10 min) and collected. Finally, the modified silica nanoparticles ① and ② were obtained by washing and drying with acetone.
[0097] (2) With the mechanical disperser agitator turned on at 1000 r / min, 27 g of environmentally friendly diluent dimethyl butanedicarboxylate, 54 g of hydroxy fluororesin JF-3X, 1 g of wetting dispersant BYK-111, 3.0 g of modified silica nanoparticles ①, 3.0 g of modified silica nanoparticles ② and 12 g of amino silicone oil OFX-8209A were added in sequence, and stirring was continued for 30 min to obtain component A modified fluororesin.
[0098] (3) 6.0 g HDI trimer, 13 g environmentally friendly diluent butyl carbonate, 0.5 g leveling agent BYK-300, and 0.5 g defoaming agent BYK-085 were added to a beaker in sequence, and stirred at 2000 r / min for 10 min at room temperature to obtain a B component curing system.
[0099] (4) Component A and component B were placed in a resonant acoustic mixing device at a mass ratio of 5:1, and treated for 30 minutes at a frequency of 150 Hz and an amplitude of 2.0 mm to obtain a mixed solution.
[0100] (5) Spray the mixed solution onto the treated glass substrate, with a coating thickness of 2.0 mm, a single-pass coating thickness of 0.8 mm, and two passes. The spraying process conditions are: air pressure 0.6 MPa, a distance of 20 cm between the spray gun and the substrate, a spraying time of 10 s, and uniform coating to obtain a super-wear-resistant and super-hydrophobic coating.
[0101] Comparative Example 3-1
[0102] A method for preparing a super-hydrophobic coating comprises the following steps:
[0103] Under the condition of opening the mechanical dispersing stirrer at 1000r / min, 27g of environmentally friendly diluent dimethyl butanedicarboxylate, 54g of hydroxy fluororesin JF-3X, 1g of dispersant BYK-111, 3.0g of modified silica nanoparticles ① (model 999121), 3.0g of modified silica nanoparticles ② (model 989213) and 12g of amino silicone oil OFX-8209A were added in sequence, and stirring was continued for 30min to obtain component A modified fluororesin; 6.0g of HDI trimer, 13g environmentally friendly diluent butyl carbonate, 0.5g leveling agent BYK-300, 0.5g defoamer BYK-085, 2000r / min stirring at room temperature for 10min to obtain component B curing system;Component A and component B are put into a resonant sound mixing device according to a mass ratio of 5: 1, and under the conditions of frequency 150Hz and amplitude 2.0mm, 30min is processed to obtain a mixed solution. The mixed solution is sprayed on the same base surface as Example 3 according to the same process parameters as Example 3 to obtain a super wear-resistant super hydrophobic coating.
[0104] Comparative Example 3-2
[0105] A method for preparing a super-hydrophobic coating comprises the following steps:
[0106] 3g of silica nanoparticles ① (model 999121) / silica microparticles (model S5505) and acetone (100mL) were added to a 250mL round-bottom flask and ultrasonically dispersed for 30min. Then, γ-aminopropylmethyldimethoxysilane (YDH-660, 1g) was added to the reaction bottle, and after electromagnetic stirring for 2h, the solid precipitate was centrifuged (2000r / min, 10min) and collected. Finally, the modified silica nanoparticles ① and modified silica microparticles were obtained by washing and drying with acetone.
[0107] Under the condition that the mechanical dispersing stirrer is turned on at 1000r / min, 27g of environmentally friendly diluent dimethyl butanedicarboxylate, 54g of hydroxy fluororesin JF-3X, 1g of dispersant BYK-111, 3.0g of modified silica nanoparticles①, 3.0g of modified silica microparticles and 12g of amino silicone oil OFX-8209A are added in sequence, and stirring is continued for 30min to obtain component A modified fluororesin; 6.0g of HDI trimer, 13g of environmentally friendly diluent butyl carbonate, 0.5g of leveling agent BYK-300 and 0.5g of defoaming agent BYK-085 are added in sequence in a beaker, and stirred at 2000r / min for 10min at room temperature to obtain component B curing system; component A and component B are put into a resonant acoustic mixing equipment at a mass ratio of 5:1, and treated for 30min at a frequency of 150Hz and an amplitude of 2.0mm to obtain a mixed solution. The mixed liquid was sprayed onto the same base surface as in Example 2 according to the same process parameters as in Example 3 to obtain a coating.
[0108] Table 1 Test results of super wear-resistant transparent super hydrophobic coatings of the embodiments and comparative examples
[0109] <![CDATA[Water contact angle( o )]]> <![CDATA[Rolling Angle( o )]]> Number of peeling Light transmittance (%) Example 1 160.2 3.2 200 92.3 Comparative Example 1-1 158.1 5.8 45 86.2 Comparative Example 1-2 159.8 4.9 150 64.6 Example 2 166.5 2.3 500 93.5 Comparative Example 2-1 161.1 3.5 70 89.3 Comparative Example 2-2 164.5 3.8 280 63.6 Example 3 160.2 4.3 300 89.5 Comparative Example 3-1 157.8 3.6 55 88.3 Comparative Example 3-2 157.5 5.2 120 68.6
[0110] Then the transmittance of the above obtained coating is tested by UV-Vis spectrophotometer, by stripping test, and the contact angle and rolling angle are measured to characterize the wear resistance of the coating, and the test results are shown in Table 1. The contact angle of the coating to water is measured by stripping test and SDC-100 model contact angle meter to characterize the wear resistance of the coating. During determination, 10 μL of water or n-hexane is dropped on the surface of the material using a contact angle meter, and the contact angles of 5 points at 4 corners and the center of the substrate are measured, and the average value is taken as the contact angle value of this plate; In order to judge the super-hydrophobic performance of the following embodiments and comparative examples. By the change of its contact angle value with the number of stripping times, its change trend diagram is drawn, and the wear resistance of its super-hydrophobic coating is judged, and the test results are shown in Table 1.
[0111] As can be seen from Table 1 above, the static water contact angle of the super wear-resistant super hydrophobic coating obtained in Examples 1 to 3 can be increased to 166.5°. Compared with Comparative Example 1-1, Comparative Example 2-1 and Comparative Example 3-1, the wear resistance of the coating in Example 1, Example 2 and Example 3 can be significantly improved, indicating that the modified silica nano ①, and modified silica nano ② and amino silicone oil can be grafted into the resin matrix by the covalent bond strategy to significantly improve the wear resistance of the super hydrophobic coating.
[0112] The transparency of the coating in Example 1, Example 2 and Example 3 is higher, which can be increased to more than 89%, indicating that by using two different particle sizes of silicon dioxide nanoparticles, a suitable roughness can be formed on the surface of the coating (reference Figure 1 ), so that the coating maintains super hydrophobicity and has excellent transparency. In Comparative Examples 1-2, 2-2 and 3-2, which use silica microparticles with larger particle sizes (particle size 200-300nm), the coating surface has a larger roughness (reference Figure 5 ), resulting in a super-hydrophobic coating with a transparency of less than 75%. The particle size of silicon dioxide has a significant effect on the light transmittance of the coating.
[0113] Among the above embodiments, Embodiment 2 is the best embodiment.
Claims
1. A method for preparing a super wear-resistant transparent super hydrophobic coating, characterized in that: The following steps are involved: Step 1: Mix hydroxy fluororesin, amino silicone oil, modified silica nanoparticles 1, modified silica nanoparticles 2, a wetting dispersant and an environmentally friendly diluent to obtain a modified fluororesin, wherein the particle size of silica in the modified silica nanoparticles 1 is 10 to 20 nm, and the particle size of silica in the modified silica nanoparticles 2 is 50 to 100 nm; Step 2, mixing a curing agent, an environmentally friendly diluent, a leveling agent, and a defoaming agent to obtain an active hydrogen-containing resin; Step 3, resonantly mixing the modified fluororesin and the active hydrogen-containing resin to obtain a mixed solution; Step 4: spray the mixed solution onto the base surface to obtain an ultra-wear-resistant, transparent, and ultra-hydrophobic coating.
2. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 1, the mass ratio of hydroxy fluororesin, amino silicone oil, modified silica nanoparticle 1, modified silica nanoparticle 2, wetting dispersant, and environmentally friendly diluent is 54:10-12:5:1-3:1-3:25.5-29.
3. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 1, the preparation methods of the modified silica nanoparticles 1 and the modified silica nanoparticles 2 are the same. The preparation method of the modified silica nanoparticles 1 is: after ultrasonically dispersing silica and acetone, adding γ-aminopropylmethyldimethoxysilane, the mass ratio of γ-aminopropylmethyldimethoxysilane to silica is 1:1 to 1:5, centrifuging and collecting the solid precipitate after electromagnetic stirring, and finally washing and drying with acetone.
4. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 1, the hydroxy fluororesin is any one of GK570, JF-2X, and JF-3X, the amino silicone oil is any one of HY-2300, OFX-8040A, and OFX-8209A, the wetting and dispersing agent is any one of BYK-111, BYK-163, BYK-220s, and BYK-P104s, and the environmentally friendly diluent is any one of propyl carbonate, dimethyl succinate, and butyl carbonate.
5. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 1, the stirring speed is 2000-2200 r / min, and the stirring time is 10-15 min.
6. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 2, the mass ratio of the curing agent, the environmentally friendly diluent, the leveling agent and the defoaming agent is 6-10:9-13:0.5:0.
5.
7. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 2, the curing agent is any one of HDI, N3390, and HDI trimer, the environmentally friendly diluent is any one of propylene carbonate, dimethyl succinate, and butyl carbonate, the leveling agent is any one of BYK300, BYK306, and BYK333, and the defoaming agent is any one of AF-8014, BYK-085, and BYK-088.
8. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step three, the mixed solution is a monodisperse mixture, and the particle size is less than 100 nm.
9. The method for preparing a super wear-resistant transparent super hydrophobic coating according to claim 1, characterized in that: In the step 4, the spraying air pressure is 0.5-0.6 MPa, the distance between the spray gun and the base surface is 15-20 cm, and the spraying time is 10-15 s.
10. A super wear-resistant transparent super hydrophobic coating obtained by the preparation method of a super wear-resistant transparent super hydrophobic coating according to any one of claims 1 to 9, characterized in that: The light transmittance is 89.5~93.5%.
Citation Information
Patent Citations
Transparent super-hydrophobic coating and preparation method thereof
CN106517821A
Preparation method of highly transparent wear-resistant superhydrophobic composite coating
CN107022279A
Transparent super-hydrophobic coating as well as preparation method and application thereof
CN108101385A
Anti-ultraviolet super-hydrophobic fluorosilicone coating as well as preparation method and application thereof
CN114854311A
Super-wear-resistant super-hydrophobic coating as well as preparation method and application thereof
CN114958174A