Water-based silver paint with excellent aluminum powder arrangement and good storage stability and preparation method of water-based silver paint

By using phosphate modified resin and amino resin to wrap aluminum powder in aqueous amino high-temperature baking silver coating, combined with directional additives, the problems of unsatisfactory aluminum powder arrangement and poor storage stability on the metal substrate are solved. , achieving low-cost and high-stability silver paint film effect.

CN118931282APending Publication Date: 2024-11-12BAZHOU MEINUO PAINT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411169228.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing water-based aluminum powder coatings are not arranged ideally after spraying on metal substrates, which are prone to blackening, and have poor storage stability and are difficult to promote wrapping aluminum powder with higher cost.

Method used

The silver coating is baked with aqueous amino high temperature, and the aluminum powder is wrapped with a special resin modified by phosphate, combined with amino resin and directional additives to avoid the reaction of aluminum powder with water, and maintain excellent aluminum powder arrangement and storage stability.

Benefits of technology

The excellent arrangement and high storage stability of aluminum powder in water-based coatings are achieved, ensuring that the product does not change color at room temperature for at least one year and is at a low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008690470000051
    Figure BDA0005008690470000051
  • Figure BDA0005008690470000061
    Figure BDA0005008690470000061
  • Figure BDA0005008690470000071
    Figure BDA0005008690470000071
Patent Text Reader

Abstract

The invention discloses water-based silver paint with excellent aluminum powder arrangement and good storage stability and a preparation method of the water-based silver paint. At normal pressure and room temperature, water-based acrylic resin, a cosolvent and a pH regulator are added into a material tank and uniformly stirred for later use; and taking another material tank, adding amino resin, aluminum powder passivation resin, a cosolvent and a pH regulator into the material tank, uniformly stirring, adding aluminum powder under the condition of keeping stirring, fully stirring and passivating, adding the mixture into the acrylic resin mixture under low-speed stirring, adding the aluminum powder directional assistant semi-finished product and other assistants, and uniformly stirring. After the coating is sprayed, the aluminum powder is excellent in arrangement, and a very good metal feeling is shown; the aluminum powder used for a traditional solvent type system with low cost is used, the aluminum powder is wrapped by special resin, the metallic feeling is not affected, reaction of water and the aluminum powder is avoided, the storage stability of the product is prolonged, and the storage shelf life of the product is at least one year.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and more specifically, to a water-based aluminum powder coating with excellent aluminum powder arrangement and good storage stability, which can be stored at room temperature for at least one year without color and gloss changes. Background Art

[0002] Water-based paint is a paint that uses water as a solvent or dispersion medium, including water-soluble paint, water-dilutable paint, water-dispersible paint, etc. It has the advantages of saving resources, eliminating the risk of construction fires, reducing air pollution, and improving the working environment, and only uses a small amount of low-toxic alcohol ether organic solvents. Water-based paint can be applied to a variety of materials such as wood, metal, plastic, glass, and building surfaces. In the field of metal substrates, such as automobiles, heavy machinery, rail transit, electric vehicles, tricycles, bicycles, etc., with the improvement of environmental awareness and the relevant environmental protection requirements issued by the state, the application of water-based paint is becoming more and more extensive. In the relevant fields of metal substrates, silver paint is a very common color paint. Silver paint uses aluminum powder as a color pigment to provide a silver visual effect. However, aluminum powder is a very active metal and it is easy to react with water. After reacting with water, hydrogen is produced, and the aluminum powder turns black and discolored. On the one hand, the hydrogen formed will expand and is a flammable gas, which is dangerous. On the other hand, the color of the paint film obtained after the aluminum powder turns black and discolored changes, and the original color paint effect cannot be achieved. At present, there is a packaged aluminum powder on the market, which has been modified and can be directly used in water-based paints, but the cost is very high and it is difficult to promote in the field of ordinary industrial paints. In addition, due to the slow evaporation rate of water, the arrangement of aluminum powder after spraying water-based aluminum powder paint is not ideal, and the resulting paint film has a poor metallic feel and is easy to turn black. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a water-based amino high-temperature baking silver paint. After the paint is sprayed, the aluminum powder is excellently arranged and shows a very good metallic feel. The aluminum powder used in the traditional solvent-based system with low usage cost is wrapped with a special resin, which does not affect the metallic feel and avoids the reaction between water and aluminum powder, thereby extending the storage stability of the product. The product has a storage shelf life of at least one year.

[0004] The technical purpose of the present invention is achieved through the following technical solutions.

[0005] A water-based silver paint with excellent aluminum powder arrangement and good storage stability and a preparation method thereof are prepared according to the following steps:

[0006] Step 1, at room temperature and normal pressure, add water-based acrylic resin, a first part of co-solvent, and a first part of pH adjuster into a first reaction container, stir evenly, and then set aside;

[0007] In step 1, the water-based acrylic resin refers to an emulsion type water-based acrylic resin or an acrylic resin that can be miscible with water in any proportion after being neutralized with an amine neutralizer, contains a certain amount of hydroxyl groups, preferably the hydroxyl content is 0.5%-2%, and the number average molecular weight of the water-based acrylic resin is between 50,000 and 200,000, preferably 80,000-150,000.

[0008] In step 1, the stirring speed is 500-800 revolutions per minute.

[0009] Step 2, at room temperature and normal pressure, add the amino resin, aluminum powder passivator, the second part of the cosolvent, and the second part of the pH adjuster into the second reaction container and stir evenly, add aluminum powder while maintaining stirring, and stir for passivation;

[0010] In step 2, the aluminum powder is conventional solvent-based aluminum powder, which is an aluminum powder slurry formed by tiny aluminum flakes dispersed in a solvent. The aluminum powder particle size is 5-40 microns, and the aluminum powder solid content is 50-80wt%.

[0011] In step 2, the amino resin refers to a melamine resin, which is a resin that can react with a hydroxyl resin, and a partially etherified or fully etherified melamine resin is selected, such as methyl etherified and / or butyl etherified; wherein based on the dry weight of the water-based acrylic resin and the amino resin, the weight ratio (amino ratio) of the acrylic resin to the amino resin is (4-8):1, preferably (5-6):1.

[0012] In step 2, the aluminum powder passivator refers to a phosphate-modified special resin, such as a phosphate-modified acrylic-styrene copolymer resin, a phosphate-modified alkyd resin, and contains 1-3% phosphorus. The phosphate radical partially rivets onto the aluminum powder, wraps the aluminum powder, isolates it from water, and stabilizes the aluminum powder without reducing the gloss and arrangement of the aluminum powder.

[0013] In step 2, the amount of the second part of the pH regulator is 20-40% of the mass of the aluminum powder passivator, preferably 20-30%; the amount of the remaining pH regulator is the amount of the first part of the pH regulator in step 1.

[0014] In step 2, the ratio of the amount of the second part of the co-solvent to the amount of the first part of the co-solvent in step 1 is (1-1.6):1.

[0015] In step 2, the stirring speed is 500-800 revolutions per minute, and the passivation time is 30-60 minutes.

[0016] In step 2, the amount of aluminum powder passivator used is 20-30wt% of the aluminum powder mass, calculated based on the solid content.

[0017] Step 3, at room temperature and normal pressure, add the passivated aluminum powder mixture obtained in step 2 to the acrylic resin mixture obtained in step 1 under low-speed stirring, and then add the aluminum powder directional auxiliary agent semi-finished product, water and other additives and stir evenly; wherein the preparation method of the aluminum powder directional auxiliary agent semi-finished product is as follows: under high-speed dispersion, add the aluminum powder directional auxiliary agent into water, and disperse it at high speed for use.

[0018] In step 3, when preparing the semi-finished aluminum powder orientation aid, the amount of water used is 25-62% of the total water used, preferably 25-50%.

[0019] In step 3, the low speed stirring is 100-300 revolutions per minute.

[0020] In step 3, the high-speed dispersion is 1000-1200 revolutions per minute, and the high-speed dispersion time is 30-60 minutes.

[0021] In step 3, the aluminum powder qualitative aid refers to a natural or synthetic silicate material that can form a house of cards type network structure in water, such as lithium magnesium silicate.

[0022] In the entire preparation scheme, the water-based acrylic resin is 20-30 parts by mass, the aluminum powder is 2-10 parts by mass, the amino resin is 2-6 parts by mass, the pH adjuster is 0.5-2 parts by mass, the water is 25-55 parts by mass, the cosolvent is 5-20 parts by mass, the aluminum powder directional aid is 0.3-2 parts by mass, the aluminum powder passivation resin is 0.5-3 parts by mass, and other additives are 0.5-1 parts by mass.

[0023] In the above technical solution, normal pressure is a standard atmospheric pressure.

[0024] In the above technical solution, the room temperature is 20-25 degrees Celsius.

[0025] In the above technical solution, the stirring and dispersing and / or dispersion adopts a mechanical stirrer or a pneumatic stirrer.

[0026] Water is selected as the dispersion medium, and a co-solvent is added at the same time. The auxiliary water is used as the solvent of the dispersion medium, which usually has good water solubility and good compatibility with water-soluble resins. A single co-solvent or multiple co-solvents are selected and blended in any proportion for use; the co-solvent is an alcohol substance, an alcohol ether substance or an alcohol ether ester substance, such as ethanol, isopropanol, n-butanol, isobutanol; propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether; ethylene glycol hexyl ether; propylene glycol methyl ether acetate, ethylene glycol butyl ether acetate or alcohol ester twelve.

[0027] Other additives are wetting agents, defoaming agents or leveling agents. One of the three components can be used alone or multiple components can be mixed in any proportion for use.

[0028] The water-based silver paint of the present invention shows excellent aluminum powder arrangement characteristics, high gloss and strong metallic feel. It also has excellent storage stability. After heat storage at 50°C for 30 days, the aluminum powder does not turn black, and the color difference between the sprayed color and the color before heat storage is ΔE≤1. It can be directly sprayed on electrophoretic paint or metal, showing good adhesion. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0030] Water-based silver paint can be used as a color paint, and then coated with varnish or as a natural color topcoat, and used directly without coating with varnish. Silver paint generally uses aluminum powder as a pigment. Well-oriented aluminum powder can show good gloss and metallic feel. Since aluminum powder reacts with water, it cannot be directly applied to water-based coatings. The present invention uses a phosphate-modified resin as a passivation resin for aluminum powder to protect the aluminum powder, and at the same time adds a directional additive to help the aluminum powder be spread flat in the paint film, which has a good reflective effect and shows an excellent metallic feel. The water-based silver paint of the present invention can be used for a variety of substrates, with or without varnish.

[0031] The acrylic resin is an emulsion acrylic resin or a water-soluble acrylic resin (i.e., the acrylic resin in the embodiment table) obtained through commercial channels. The emulsion acrylic resin is such as VSC 6276W, SETAQUA6160 of Allnex, and 5914K of Huaguoshan Chemical; the water-soluble acrylic resin is such as DA066 of Shenghui Chemical, or SW-119 of Sanwang Chemical.

[0032] Aluminum powder passivators are available through commercial channels, such as Lubrizol 2062H, Shenghui Chemical 6040, 6005.

[0033] Aluminum powder was obtained through commercial channels, conventional aluminum powder used in traditional oily products, with no special model specified.

[0034] Amino resins are obtained through commercial channels, such as CYMEL325, CYMEL327, CYMEL303 from Allnex; N0086, N0087, N0089 from Tianhong Trading; or 5817, 5819 from Sanmu Chemical.

[0035] Aluminum powder directing agents are available through commercial channels, such as BYK's RD and RDS.

[0036] Water is selected as the dispersion medium, and a co-solvent is added at the same time. The solvent of the auxiliary water as the dispersion medium usually has good water solubility and good compatibility with alcohol-soluble resins, and is an alcohol substance, an alcohol ether substance or an alcohol ether ester substance, such as ethanol, isopropanol, n-butanol, isobutanol; propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, ethylene glycol hexyl ether, diethylene glycol butyl ether; propylene glycol methyl ether acetate, ethylene glycol butyl ether acetate or alcohol ester twelve.

[0037] In addition, other additives are added and obtained through commercial channels, such as wetting agents, which provide good wetting and spreading properties of the water-based silver paint on the substrate or primer; leveling agents, which improve flow and leveling and increase the flatness of the water-based silver paint film; defoaming agents, which inhibit the formation of bubbles and make the generated bubbles escape or burst during the production process and product construction process; pH adjusters, which are used to neutralize the passivation resin and adjust the pH value of the resin or the finished paint to improve storage stability.

[0038] The water-based silver paint 1-4 of the present invention is prepared by the following preparation method: add acrylic resin to a material tank and start stirring, add a cosolvent (the first part) and a pH regulator (the first part) under medium-speed stirring, and continue stirring for 20-30 minutes for standby, so as to obtain an acrylic resin mixture. Take another material tank, add amino resin, aluminum powder passivator (aluminum powder passivation resin in the table below), and a cosolvent (the second part) and start stirring, add a pH regulator (the second part) under medium-speed stirring and continue stirring for 10 minutes, and further, add aluminum powder while maintaining stirring, and fully stir and passivate for 40 minutes. Add the passivated aluminum powder mixture to the acrylic resin mixture under low-speed stirring, and then add a semi-finished aluminum powder directional auxiliary agent (aluminum powder directional auxiliary agent in the table below), water and other auxiliary agents and stir evenly. The preparation method of the semi-finished aluminum powder directional auxiliary agent is as follows: under 800-1000 rpm high-speed dispersion, add the aluminum powder directional agent to water, disperse at high speed for 30 minutes, and set aside.

[0039] The desired water-based silver paints 1-4 were thus obtained, and the components and amounts of each composition are listed in the following Tables 1-4.

[0040] Table 1: Components and dosage of water-based silver paint-1

[0041] Components Component function Weight: 1kg per portion VSC 6276W Acrylic resin 40 Ethylene glycol butyl ether Cosolvents (Part 1) 5 Dimethylethanolamine pH Adjusters (Part 1) 0.3 CYMEL325 Amino resin 5.41 Ethylene glycol hexyl ether Cosolvents (Part 2) 8 2062H Aluminum powder passivation resin 2.8 Dimethylethanolamine pH Adjusters (Part 2) 0.6 Aluminum powder Silver Pigment 10 water Dispersion medium 20 RD Aluminum powder directional additive 0.4 water Dispersion medium (preparation of aluminum powder directional additive semi-finished products) 6.99 TEGO-270 Wetting Agents 0.3 TEGO-810 Defoaming agent 0.2

[0042] Note: The amino ratio is 5:1, based on the weight ratio of the dry weight of the water-based acrylic resin and the amino resin. The solid content of the emulsion acrylic resin in the present invention is 45wt%, the solid content of the water-soluble acrylic resin is 70wt%, and the solid content of the amino resin is 70-80wt%. VOC < 420g / L, measured according to GB / T23985 8.4.

[0043] Table 2: Components and dosage of water-based silver paint-2

[0044]

[0045]

[0046] Note: The amino ratio is 8:1. VOC<420g / L.

[0047] Table 3: Components and dosage of water-based silver paint-3

[0048] Components Component function Weight: 1kg per portion DA066 Acrylic resin 20 n-Butanol Cosolvents (Part 1) 8 Dimethylethanolamine pH Adjusters (Part 1) 1 5817 Amino resin 5 Propylene glycol methyl ether Cosolvents (Part 2) 10 6005 Aluminum powder passivation resin 0.5 Dimethylethanolamine pH Adjusters (Part 2) 0.2 Aluminum powder Silver Pigment 2 water Dispersion medium 30 RD Aluminum powder directional additive 0.6 water Dispersion medium (preparation of aluminum powder directional additive semi-finished products) 22.2 BYK-348 Wetting Agents 0.3 BYK-024 Defoaming agent 0.2

[0049] Note: Amino ratio is 4:1. VOC<420g / L, measured according to GB / T23985 8.4.

[0050] Table 4: Components and weights of water-based silver paint-4

[0051]

[0052]

[0053] Note: Amino ratio is 6:1. VOC<420g / L, measured according to GB / T23985 8.4.

[0054] Performance Testing

[0055] Water-based silver paint was applied to the black electrophoretic primer coated on the tinplate for testing. Water-based silver paint 1-4 was sprayed onto the prepared substrate with a conventional air spray gun, and after 10 minutes of surface drying at room temperature, it was baked at 140°C for 20 minutes, with a dry film thickness of 15-25 microns, and the five-angle color difference reaction arrangement effect was tested. The paint was placed in a 50°C oven for 30 days and then the sample was re-sprayed to test the storage stability of the 45° color difference reaction paint before and after thermal storage. The test results are as follows:

[0056]

[0057]

[0058] It can be seen from the results that the water-based silver paint 1-4 of the present invention shows a very high L value at the front angle, i.e., a small angle, and a lower L value at the side angle, i.e., a large angle, indicating that the aluminum powder is arranged very well and the front is very bright. The color difference values ​​ΔE before and after hot storage are both less than 1, showing the excellent storage stability of the aluminum powder. The product is stored for more than one year at room temperature and the aluminum powder does not turn black. The water-based silver paint of the present invention also meets the national standard requirements for water-based paints and meets the standards for water-based paints. The water-based silver paint of the present invention has good application prospects in metal parts, such as the tricycle industry, the automotive parts industry and other fields.

[0059] According to the content of the present invention, the process parameters can be adjusted to achieve the preparation of the coating, and after testing, the coating exhibits performance substantially consistent with the present invention. The present invention is described above by way of example, and it should be noted that any simple deformation, modification or equivalent replacement that can be made by other technicians in this field without inventive labor falls within the protection scope of the present invention without departing from the core of the present invention.

Claims

1. A water-based silver paint with excellent aluminum powder arrangement and good storage stability, characterized in that: The water-based acrylic resin is 20-30 parts by mass, the aluminum powder is 2-10 parts by mass, the amino resin is 2-6 parts by mass, the pH adjuster is 0.5-2 parts by mass, the water is 25-55 parts by mass, the cosolvent is 5-20 parts by mass, the aluminum powder directional auxiliary agent is 0.3-2 parts by mass, the aluminum powder passivation resin is 0.5-3 parts by mass, and other auxiliary agents are 0.5-1 parts by mass. The preparation is carried out according to the following steps: Step 1, at room temperature and normal pressure, add water-based acrylic resin, a first part of co-solvent, and a first part of pH adjuster into a first reaction container, stir evenly, and then set aside; In step 1, the water-based acrylic resin refers to an emulsion type water-based acrylic resin or an acrylic resin that can be miscible with water in any proportion after being neutralized with an amine neutralizer, the hydroxyl content is 0.5%-2%, and the number average molecular weight of the water-based acrylic resin is between 50000 and 200000; Step 2, at room temperature and normal pressure, add the amino resin, aluminum powder passivator, the second part of the cosolvent, and the second part of the pH adjuster into the second reaction container and stir evenly, add aluminum powder while maintaining stirring, and stir for passivation; In step 2, the aluminum powder is a traditional solvent aluminum powder, which is an aluminum powder slurry formed by tiny aluminum flakes dispersed in a solvent, with a particle size of 5-40 microns and a solid content of 50-80wt%; the amino resin refers to a melamine resin, which is a resin that can react with a hydroxyl resin, and a partially etherified or fully etherified melamine resin is selected; wherein based on the dry weight of the water-based acrylic resin and the amino resin, the weight ratio (amino ratio) of the acrylic resin and the amino resin is (4-8): 1; the aluminum powder passivator refers to a phosphate-modified special resin with a phosphorus content of 1-3%. The phosphate radical is partially riveted to the aluminum powder, wrapping the aluminum powder and isolating it from water, thereby stabilizing the aluminum powder without reducing the gloss and arrangement of the aluminum powder; the amount of the second part of the pH regulator is 20-40% of the mass of the aluminum powder passivator, and the amount of the remaining pH regulator is the amount of the first part of the pH regulator in step 1; the amount of the aluminum powder passivator is 20-30wt% of the mass of the aluminum powder, calculated based on the solid content; Step 3, under normal pressure and room temperature, add the passivated aluminum powder mixture obtained in step 2 to the acrylic resin mixture obtained in step 1 under low-speed stirring, and then add the aluminum powder directional auxiliary agent semi-finished product, water and other auxiliary agents and stir evenly; wherein the preparation method of the aluminum powder directional auxiliary agent semi-finished product is as follows: under high-speed dispersion, add the aluminum powder directional auxiliary agent into water, and disperse at high speed for use; In step 3, the aluminum powder directional additive refers to a natural or synthetic silicate material that can form a card house type network structure in water, such as lithium magnesium silicate; when preparing the aluminum powder directional additive semi-finished product, the amount of water used is 25-62% of the total water used.

2. The water-based silver paint with excellent aluminum powder arrangement and good storage stability according to claim 1, characterized in that: In step 1, the number average molecular weight of the water-based acrylic resin is 80,000-150,000, and the stirring speed is 500-800 revolutions per minute; in step 3, when preparing the aluminum powder directional auxiliary agent semi-finished product, the amount of water used is 25-50% of the total water amount, the low-speed stirring is 100-300 revolutions per minute; the high-speed dispersion is 1000-1200 revolutions per minute, and the high-speed dispersion time is 30-60 minutes.

3. The water-based silver paint with excellent aluminum powder arrangement and good storage stability according to claim 1, characterized in that: In step 2, the amino resin refers to methyl etherified and / or butyl etherified melamine resin, and the weight ratio (amino ratio) of the acrylic resin to the amino resin is (5-6):1 based on the dry weight of the water-based acrylic resin and the amino resin; the aluminum powder passivator refers to a phosphate-modified acrylic-styrene copolymer resin, or a phosphate-modified alkyd resin; the amount of the second part of the pH regulator is 20-30% of the mass of the aluminum powder passivator, and the amount of the remaining pH regulator is the amount of the first part of the pH regulator in step 1; the ratio of the amount of the second part of the co-solvent to the amount of the first part of the co-solvent in step 1 is (1-1.6):1; the stirring speed is 500-800 revolutions per minute, and the passivation time is 30-60 minutes.

4. The water-based silver paint with excellent aluminum powder arrangement and good storage stability according to claim 1, characterized in that: Normal pressure is a standard atmospheric pressure, and room temperature is 20-25 degrees Celsius; stirring and / or dispersing uses a mechanical stirrer or a pneumatic stirrer; other additives are wetting agents, defoaming agents or leveling agents, and one of the three components is selected for use alone or multiple components are blended in any proportion.

5. The water-based silver paint with excellent aluminum powder arrangement and good storage stability according to claim 1, characterized in that: Water is selected as the dispersion medium, and a co-solvent is added at the same time to assist water as the solvent of the dispersion medium. A single co-solvent or multiple co-solvents are selected and blended in any proportion for use; the co-solvent is an alcohol substance, an alcohol ether substance or an alcohol ether ester substance, such as ethanol, isopropanol, n-butanol, isobutanol; propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether; ethylene glycol hexyl ether; propylene glycol methyl ether acetate, ethylene glycol butyl ether acetate or alcohol ester twelve.

6. A method for preparing a water-based silver paint having excellent aluminum powder arrangement and good storage stability, characterized in that: The water-based acrylic resin is 20-30 parts by mass, the aluminum powder is 2-10 parts by mass, the amino resin is 2-6 parts by mass, the pH adjuster is 0.5-2 parts by mass, the water is 25-55 parts by mass, the cosolvent is 5-20 parts by mass, the aluminum powder directional auxiliary agent is 0.3-2 parts by mass, the aluminum powder passivation resin is 0.5-3 parts by mass, and other auxiliary agents are 0.5-1 parts by mass. The preparation is carried out according to the following steps: Step 1, at room temperature and normal pressure, add water-based acrylic resin, a first part of co-solvent, and a first part of pH adjuster into a first reaction container, stir evenly, and then set aside; In step 1, the water-based acrylic resin refers to an emulsion type water-based acrylic resin or an acrylic resin that can be miscible with water in any proportion after being neutralized with an amine neutralizer, the hydroxyl content is 0.5%-2%, and the number average molecular weight of the water-based acrylic resin is between 50000 and 200000; Step 2, at room temperature and normal pressure, add the amino resin, aluminum powder passivator, the second part of the cosolvent, and the second part of the pH adjuster into the second reaction container and stir evenly, add aluminum powder while maintaining stirring, and stir for passivation; In step 2, the aluminum powder is a traditional solvent aluminum powder, which is an aluminum powder slurry formed by tiny aluminum flakes dispersed in a solvent, with a particle size of 5-40 microns and a solid content of 50-80wt%; the amino resin refers to a melamine resin, which is a resin that can react with a hydroxyl resin, and a partially etherified or fully etherified melamine resin is selected; wherein based on the dry weight of the water-based acrylic resin and the amino resin, the weight ratio (amino ratio) of the acrylic resin and the amino resin is (4-8): 1; the aluminum powder passivator refers to a phosphate-modified special resin with a phosphorus content of 1-3%. The phosphate radical is partially riveted to the aluminum powder, wrapping the aluminum powder and isolating it from water, thereby stabilizing the aluminum powder without reducing the gloss and arrangement of the aluminum powder; the amount of the second part of the pH regulator is 20-40% of the mass of the aluminum powder passivator, and the amount of the remaining pH regulator is the amount of the first part of the pH regulator in step 1; the amount of the aluminum powder passivator is 20-30wt% of the mass of the aluminum powder, calculated based on the solid content; Step 3, under normal pressure and room temperature, add the passivated aluminum powder mixture obtained in step 2 to the acrylic resin mixture obtained in step 1 under low-speed stirring, and then add the aluminum powder directional auxiliary agent semi-finished product, water and other auxiliary agents and stir evenly; wherein the preparation method of the aluminum powder directional auxiliary agent semi-finished product is as follows: under high-speed dispersion, add the aluminum powder directional auxiliary agent into water, and disperse at high speed for use; In step 3, the aluminum powder directional additive refers to a natural or synthetic silicate material that can form a card house type network structure in water, such as lithium magnesium silicate; when preparing the aluminum powder directional additive semi-finished product, the amount of water used is 25-62% of the total water used.

7. The method for preparing a water-based silver paint having excellent aluminum powder arrangement and good storage stability according to claim 6, characterized in that: In step 1, the number average molecular weight of the water-based acrylic resin is 80,000-150,000, and the stirring speed is 500-800 revolutions per minute; in step 3, when preparing the aluminum powder directional auxiliary agent semi-finished product, the amount of water used is 25-50% of the total water amount, the low-speed stirring is 100-300 revolutions per minute; the high-speed dispersion is 1000-1200 revolutions per minute, and the high-speed dispersion time is 30-60 minutes.

8. The method for preparing a water-based silver paint having excellent aluminum powder arrangement and good storage stability according to claim 6, characterized in that: In step 2, the amino resin refers to methyl etherified and / or butyl etherified melamine resin, and the weight ratio (amino ratio) of the acrylic resin to the amino resin is (5-6):1 based on the dry weight of the water-based acrylic resin and the amino resin; the aluminum powder passivator refers to a phosphate-modified acrylic-styrene copolymer resin, or a phosphate-modified alkyd resin; the amount of the second part of the pH regulator is 20-30% of the mass of the aluminum powder passivator, and the amount of the remaining pH regulator is the amount of the first part of the pH regulator in step 1; the ratio of the amount of the second part of the co-solvent to the amount of the first part of the co-solvent in step 1 is (1-1.6):1; the stirring speed is 500-800 revolutions per minute, and the passivation time is 30-60 minutes.

9. The method for preparing a water-based silver paint having excellent aluminum powder arrangement and good storage stability according to claim 6, characterized in that: Normal pressure is a standard atmospheric pressure, and room temperature is 20-25 degrees Celsius; stirring and / or dispersing uses a mechanical stirrer or a pneumatic stirrer; other additives are wetting agents, defoaming agents or leveling agents, and one of the three components is selected for use alone or multiple components are blended in any proportion.

10. The method for preparing a water-based silver paint having excellent aluminum powder arrangement and good storage stability according to claim 6, characterized in that: Water is selected as the dispersion medium, and a co-solvent is added at the same time to assist water as the solvent of the dispersion medium. A single co-solvent or multiple co-solvents are selected and blended in any proportion for use; the co-solvent is an alcohol substance, an alcohol ether substance or an alcohol ether ester substance, such as ethanol, isopropanol, n-butanol, isobutanol; propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether; ethylene glycol hexyl ether; propylene glycol methyl ether acetate, ethylene glycol butyl ether acetate or alcohol ester twelve.

Citation Information

Patent Citations

  • Method for using solvent type resin aluminum pigment in water paint

    CN101760071A

  • Directive water-based acrylic resin with excellent aluminite powder and preparation and coating thereof

    CN106478860A

  • Water-based flash colored paint and preparation method thereof

    CN110229574A

  • Oily silver paste for automobile water-based paint and automobile water-based paint

    CN110885604A

  • Water-based electric bicycle aluminium powder paint containing oily aluminum paste and preparation method thereof

    CN112126289A