Preparation method of varnish coating with building block-shaped nickel oxide nanoparticles as sealing agent

By combining building block-like nickel oxide nanoparticles with 2-mercaptobenzothiazole-efficient alkyd resin varnish, a high-performance coating is formed, and the problem of insufficient corrosion resistance of metal components in the prior art is solved, and the corrosion resistance performance in harsh environments is achieved. Low corrosion current, higher corrosion potential and larger impedance are used to significantly improve corrosion resistance.

CN118931339APending Publication Date: 2024-11-12GUANGXI UNIV FOR NATITIES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411400299.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the corrosion resistance of metal parts in harsh environments, especially since hexavalent chromium and tritetroxide are prohibited, the corrosion resistance of traditional hot water sealing methods is poor, and the existing organic sealing membrane is in harsh conditions. Limited effect in the environment.

Method used

Building block-like nickel oxide nanoparticles are used as the sealing agent, and bonded to the surface of the metal component by ultrasonication, and then covered with 2-mercaptobenzothiazole-generated alkyd resin varnish to form a high-performance coating.

Benefits of technology

It significantly reduces corrosion current, improves corrosion potential and AC impedance, enhances the resistance to brine corrosion, has better performance than traditional alkyd resin varnish coatings, and is relatively easy to make.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931339A_ABST
    Figure CN118931339A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a varnish coating taking building block-shaped nickel oxide nanoparticles as a sealing agent, and the preparation method of the coating comprises the following steps: taking the building block-shaped nickel oxide nanoparticles as the sealing agent on the surface of a metal part substrate, and then covering a layer of alkyd resin varnish with 2-mercaptobenzothiazole for synergism. The coating prepared by the method has relatively high corrosion potential, relatively low corrosion current and relatively large impedance, which indicates that the coating has relatively good corrosion resistance. The coating can be applied to anticorrosion engineering of surfaces of electrical equipment such as air conditioners, electric water heaters, air conditioners and refrigerators and metal parts of mechanical equipment such as tractors and cranes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of anti-corrosion varnish coatings, in particular to a method for preparing a varnish coating using building block-shaped nickel oxide nanoparticles as a sealing agent. Background Art

[0002] In order to improve the corrosion resistance of metal parts, the traditional method is to use heavy metals such as hexavalent chromium and lead tetroxide or hot water sealing method, and then cover a layer of coating. However, hexavalent chromium, lead tetroxide, etc. are toxic. In the electrical and electronic industries, the EU RoHS regulations (Restriction of Hazardous Substances, "Directive on Restricting the Use of Certain Hazardous Substances in Electrical and Electronic Equipment") prohibit the use of compounds such as hexavalent chromium and lead tetroxide. Although the hot water direct sealing method is non-toxic, it has poor corrosion resistance. In practical applications, especially in harsh environments, it will encounter difficult to overcome corrosion problems. The inventor's early Chinese patents "A Preparation Method for Aluminum Alloy Organic Sealing Film and Its Film-forming Solution" (Patent No.: CN201110315302.4) and "A Preparation Method for Aluminum Alloy Organic Aminophenol Composite Sealing Film and Its Film-forming Solution" (Patent No. CN 201310075903.1) have good effects, but their effects are still limited when used in harsh environments. Therefore, it is of great significance to study a method for preparing a high-performance coating that is easy to make. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a varnish coating which is easy to prepare and uses building block-shaped nickel oxide nanoparticles as a sealing agent.

[0004] In order to solve the above technical problems, the present invention adopts the following technical scheme: firstly, building block-like nickel oxide nanoparticles are synthesized, and the surface of the metal parts is sealed with the prepared building block-like nickel oxide nanoparticles, and then a layer of prepared 2-mercaptobenzothiazole-enhanced alkyd resin varnish is coated on the surface of the sealed metal parts to obtain the result.

[0005] The above-mentioned method for preparing a varnish coating with building block-like nickel oxide nanoparticles as a sealant comprises using building block-like nickel oxide nanoparticles as a sealant, immersing a metal part in the sealant and ultrasonically treating the metal part, and then covering the surface of the sealed metal part with a layer of prepared 2-mercaptobenzothiazole-enhanced alkyd resin varnish.

[0006] The above-mentioned method for preparing a varnish coating using building block-shaped nickel oxide nanoparticles as a sealing agent comprises the following steps: <1> Synthesis of building block nickel oxide nanoparticles: 0.02 mol nickel nitrate hexahydrate (Ni(NO 3 ) 2 •6H2 O), 20 ml of deionized water, 0.001 mol of sodium dodecylbenzene sulfonate dissolved in 100 ml of ethanol, slowly drop 40 ml of sodium hydroxide with a concentration of 0.0025 g / L and stir vigorously for 30 minutes, transfer the resulting solution to a reactor lined with 500 ml of polytetrafluoroethylene , The reaction was carried out at 190°C for 2 hours, and after cooling to room temperature, the precipitate was obtained by centrifugation, washed three times with deionized water and ethanol, and baked at 360°C for 1 hour. <2> Preparation of 2-mercaptobenzothiazole-enhanced alkyd resin varnish: 100 g of dry long oil alkyd resin, 0.5 g of cobalt naphthenate drier, and 2.5 g of 2-mercaptobenzothiazole are sequentially added to 50 ml of n-butanol solvent, and mechanically stirred for 5 minutes each time a chemical substance is added, and finally stirred at high speed for 5 minutes to obtain the varnish; <3> Preparation of clear coat: weighing steps <1> 0.01-0.8 g of prepared nickel oxide nanoparticles are added to 100 ml of a mixture of water and n-butyl in a volume ratio of 2:1, and ultrasonicated for 3-5 minutes. A clean metal part is immersed in the mixture to seal it, and ultrasonicated for another 3-5 minutes. After the metal part is taken out and dried, a layer of <2> The prepared varnish is dried naturally for 12 hours.

[0007] Experiments have shown that low carbon steel electrodes for The prepared building block-like nickel oxide particles were sealed with a sealant and then covered with a layer of prepared varnish. The exposed area was tested on an electrochemical workstation with an exposed area of ​​1 square centimeter. The polarization curve results showed that the corrosion current of the coating after the building block-like nickel oxide nanoparticles were sealed and covered with a layer of 2-mercaptobenzothiazole-enhanced alkyd resin varnish was the lowest, and its corrosion potential increased by 100 mV over the unsealed alkyd resin alcohol varnish coating containing 2-mercaptobenzothiazole and 200 mV over the unsealed alkyd resin alcohol varnish coating without 2-mercaptobenzothiazole. The AC impedance test results showed that the impedance of the coating after the building block-like nickel oxide nanoparticles were sealed and covered with a layer of 2-mercaptobenzothiazole-enhanced alkyd resin varnish increased by 10 kohm.cm over the unsealed alkyd resin alcohol varnish coating containing 2-mercaptobenzothiazole. 2 , more than 50 kohm.cm over an unblocked alkyd clearcoat without 2-mercaptobenzothiazole 2 The tinplate coated by this method was immersed in 3.5% sodium chloride solution for 20 days, and only slightly corroded. It exceeds the performance of the current alkyd resin varnish coating and is easy to make. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 This is a transmission electron microscope image of the prepared building block-like nickel oxide nanoparticles.

[0009] Figure 2 The polarization curves of the coatings prepared by the method for preparing a varnish coating with building block-like nickel oxide nanoparticles as a sealant in Example 1 are as follows: Curve a is an alkyd resin alcohol varnish coating without 2-mercaptobenzothiazole, Curve b is an alkyd resin alcohol varnish coating containing 2-mercaptobenzothiazole, and Curve c is an alkyd resin alcohol varnish coating sealed with a building block-like nickel oxide nanoparticle sealant and then covered with a layer of alkyd resin alcohol varnish coating enhanced with 2-mercaptobenzothiazole.

[0010] Figure 3 This is an AC impedance diagram of a coating prepared by the method for preparing a varnish coating with building block-like nickel oxide nanoparticles as a sealant in Example 1: Curve a is an alkyd resin alcohol varnish coating without 2-mercaptobenzothiazole, curve b is an alkyd resin alcohol coating containing 2-mercaptobenzothiazole, and curve c is a building block-like nickel oxide nanoparticle sealant sealed and then covered with a layer of alkyd resin alcohol varnish coating enhanced with 2-mercaptobenzothiazole.

[0011] Figure 4 This is a corrosion photograph of the alkyd resin varnish coating without 2-mercaptobenzothiazole in Example 1 immersed in a 3.5% sodium chloride solution for 20 days.

[0012] Figure 5 This is a corrosion photograph of the alkyd resin varnish coating containing 2-mercaptobenzothiazole in Example 1 immersed in a 3.5% sodium chloride solution for 20 days.

[0013] Figure 6 This is a corrosion photograph of the sample in Example 1 which was sealed with a building block-like nickel oxide nanoparticle sealant and then covered with a layer of alkyd resin varnish coating enhanced with 2-mercaptobenzothiazole and immersed in a 3.5% sodium chloride solution for 20 days. DETAILED DESCRIPTION Example

[0015] 1. Pretreatment of electrodes and tinplate sheets The electrodes (Q235 low carbon steel electrodes (1 cm in diameter) were used for electrochemical testing) and tinplate sheets (12 cm × 5 cm × 1 mm) were polished with 280-mesh and 600-mesh sandpapers, respectively. Then, they were ultrasonically cleaned in 5% hydrochloric acid for 1 min, ultrasonically cleaned in deionized water for 5 min, and finally ultrasonically cleaned in anhydrous ethanol for 5 min and dried for later use.

[0016] 2. Preparation of building block nickel oxide nanoparticles, varnish and coating film <1> Synthesis of building block nickel oxide nanoparticles: 0.02 mol nickel nitrate hexahydrate (Ni(NO 3 )2 •6H 2 O), 20 ml of deionized water, 0.001 mol of sodium dodecylbenzene sulfonate dissolved in 100 ml of ethanol, slowly drop 40 ml of sodium hydroxide with a concentration of 0.0025 g / L and stir vigorously for 30 minutes, transfer the resulting solution to a reactor lined with 500 ml of polytetrafluoroethylene , The reaction was carried out at 190°C for 2 hours, and after cooling to room temperature, the precipitate was obtained by centrifugation, washed three times with deionized water and ethanol, and baked at 360°C for 1 hour. <2> Preparation of 2-mercaptobenzothiazole-enhanced alkyd resin varnish: 100 g of dry long oil alkyd resin, 0.5 g of cobalt naphthenate drier, and 2.5 g of 2-mercaptobenzothiazole are sequentially added to 50 ml of n-butanol solvent, and mechanically stirred for 5 minutes each time a chemical substance is added, and finally stirred at high speed for 5 minutes to obtain the varnish; <3> Preparation of clear coat: weighing steps <1> 0.6 g of the prepared building block-like nickel oxide nanoparticles were added to 100 ml of a mixture of water and n-butyl in a volume ratio of 2:1, and ultrasonicated for 5 minutes. A clean metal part was immersed in the mixture to seal it, and ultrasonicated for another 5 minutes. After the metal part was taken out and dried, a layer of <2> The prepared varnish is dried naturally for 12 hours.

[0017] <4> Preparation of coating of alkyd resin varnish without 2-mercaptobenzothiazole: First, prepare the varnish, except that 2-mercaptobenzothiazole is not added, and the preparation process steps are as follows: <2> Exactly the same, then directly immerse the treated mild steel electrode or tinplate sheet into the alkyd resin varnish free of 2-mercaptobenzothiazole for 5 minutes, then take out the mild steel electrode or tinplate sheet and dry it naturally for 12 hours, thus obtaining the alkyd resin alcohol varnish coating free of 2-mercaptobenzothiazole; <5> Preparation of coating of alkyd resin varnish containing 2-mercaptobenzothiazole: Immerse the treated low carbon steel electrode or tinplate sheet in step <2> The prepared alkyd resin varnish containing 2-mercaptobenzothiazole is immersed for 5 minutes, and then the low-carbon steel electrode or tinplate sheet is taken out and naturally dried for 12 hours to obtain the alkyd resin varnish coating containing 2-mercaptobenzothiazole.

[0018] 3. Anti-corrosion performance test of coating <1> The electrodes coated with the prepared alkyd resin varnish coating without 2-mercaptobenzothiazole, the alkyd resin varnish coating containing 2-mercaptobenzothiazole, and the block-shaped nickel oxide nanoparticles were sealed and covered with a layer of alkyd resin varnish enhanced with 2-mercaptobenzothiazole, so that the exposed area of ​​the coating was 1 square centimeter. Then, electrochemical polarization curves and AC impedance tests were carried out in 3.5% sodium chloride solution to compare the corrosion current, corrosion potential and impedance. It was found that the corrosion current of the coating sealed with the block-shaped nickel oxide nanoparticles and covered with a layer of alkyd resin varnish enhanced with 2-mercaptobenzothiazole was the lowest, and its corrosion potential increased by 110 mV more than that of the unsealed alkyd resin varnish coating containing 2-mercaptobenzothiazole, and 210 mV more than that of the unsealed alkyd resin varnish coating without 2-mercaptobenzothiazole (such as Figure 2 The impedance increase is 10 kohm.cm over the unblocked alkyd resin varnish coating containing 2-mercaptobenzothiazole. 2 , more than 50 kohm.cm over an unblocked alkyd clearcoat without 2-mercaptobenzothiazole 2 ( like Figure 3 as shown).

[0019] <2> Tinplate sheets coated with the prepared alkyd resin varnish coating without 2-mercaptobenzothiazole, the alkyd resin varnish coating containing 2-mercaptobenzothiazole, the alkyd resin varnish coated with the block-like nickel oxide nanoparticles and covered with a layer of alkyd resin varnish enhanced with 2-mercaptobenzothiazole were immersed in a 3.5% sodium chloride solution for 20 days. It was found that the tinplate sheet coated with the alkyd resin varnish without 2-mercaptobenzothiazole was severely corroded (such as Figure 4 As shown); alkyd resin varnish coating containing 2-mercaptobenzothiazole, although corrosive, is slightly lighter (such as Figure 5 As shown); after being sealed with building block-like nickel oxide nanoparticles and covered with a coating of 2-mercaptobenzothiazole-enhanced alkyd resin varnish, there is only slight corrosion (such as Figure 6 as shown).

[0020] Therefore, the coating prepared by the method for preparing a varnish coating using building block-shaped nickel oxide nanoparticles as a sealing agent has a lower corrosion current, a higher corrosion potential and a larger impedance, a strong ability to resist salt water corrosion, and better anti-corrosion performance.

Claims

1. A method for preparing a varnish coating using building block-like nickel oxide nanoparticles as a sealing agent, characterized in that: The building block-like nickel oxide nanoparticles are used as a sealant on the surface of the metal parts, and after sealing, a layer of alkyd resin varnish enhanced by 2-mercaptobenzothiazole is applied; Please follow the steps below: <1> Synthesis of building block-like nickel oxide nanoparticles: 0.02 mol nickel nitrate hexahydrate (Ni(NO3)2•6H2O), 20 ml deionized water, and 0.001 mol sodium dodecylbenzene sulfonate were weighed and dissolved in 100 ml ethanol, 40 ml of 0.0025 g / L sodium hydroxide was slowly added and stirred vigorously for 30 minutes, and the resulting solution was transferred to a reactor lined with 500 ml polytetrafluoroethylene. , The reaction was carried out at 190°C for 2 hours, and after cooling to room temperature, the precipitate was obtained by centrifugation, washed three times with deionized water and ethanol, and baked at 360°C for 1 hour. <2> Preparation of 2-mercaptobenzothiazole-enhanced alkyd resin varnish: 100 g of dry long oil alkyd resin, 0.5 g of cobalt naphthenate drier, and 2.5 g of 2-mercaptobenzothiazole are sequentially added to 50 ml of n-butanol solvent, and mechanically stirred for 5 minutes each time a chemical substance is added, and finally stirred at high speed for 5 minutes to obtain the varnish; <3> Preparation of clear coat: weighing steps <1> 0.01-0.8 g of the prepared building block-like nickel oxide nanoparticles are added to 100 ml of a mixture of water and n-butyl in a volume ratio of 2:1, and ultrasonicated for 3-5 minutes. A clean metal part is immersed in the mixture to seal it, and ultrasonicated for another 3-5 minutes. After the metal part is taken out and dried, a layer of <2> The prepared varnish is dried naturally for 12 hours.

Citation Information

Patent Citations

  • Hole sealing agent, preparation method and application thereof, coating film, preparation method of coating film and anti-corrosion product

    CN111718606A

  • Anticorrosive hydrophobic antibacterial coating in seawater and preparation method ofanticorrosive hydrophobic antibacterial coating

    CN112126265A

  • Nanowires-based transparent conductors

    US20070074316A1

  • Composite nickel nanoparticles and method for producing same

    WO2012124625A1