Self-cleaning polyurethane heat insulation coating material applied to building surface and preparation method thereof
By adding modified silicone oligomers and modified nanotitanium dioxide particle solution to the polyurethane coating, the problem of poor compatibility of inorganic nanoparticles and resins is solved, the hydrophobicity and durability of the coating are improved, and the better Self-cleaning effect and flatness.
Patent Information
- Application Number
- CN202411019131.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing self-cleaning polyurethane insulating coating materials have poor self-cleaning effect and low durability. This is mainly due to the agglomeration of inorganic nanoparticles and poor resin compatibility, resulting in reduced coating flatness and surface defects, which affect hydrophobicity and weather resistance.
Using modified silicone oligomers and modified nanotitanium dioxide particle solutions, the surface energy and hydrophobicity of the coating are improved through photocatalysis and cross-linking reactions, and the dispersion and compatibility of nanoparticles are improved through modification treatment to enhance the The durability and self-cleaning capability of the coating.
It significantly improves the hydrophobicity and durability of polyurethane coatings, enhances the coating's anti-pollution ability and weather resistance, and achieves better self-cleaning effect and smoothness.
Smart Images

Figure BDA0004966671810000141 
Figure BDA0004966671810000151
Abstract
Description
Technical Field
[0001] The present application relates to the field of coating material technology, in particular to a self-cleaning polyurethane thermal insulation coating material for building surface application and a preparation method thereof. Background Art
[0002] As a polymer material with high strength, tear resistance, and wear resistance, polyurethane resin is widely used in daily life, industrial and agricultural production, medicine, and other fields. It is used for insulation and cold preservation of storage tanks, pipelines, cold storage, beer, fermentation tanks, and fresh-keeping barrels, and insulation and waterproofing of houses and buildings, etc. It has excellent waterproof properties. Building exterior wall coatings can beautify the environment and living rooms, but due to the poor scrubbing resistance of traditional coatings, the coating will change color and fall off after a short time. Glass curtain walls or tile veneers will bring light pollution, increase the weight of buildings, and pose safety hazards. And as the environmental pollution in cities is intensifying, dust pollution and gas pollution are particularly serious. The exterior walls of buildings, especially high-rise buildings, are being eroded more and more seriously. The role of self-cleaning coatings is becoming more and more important. Self-cleaning coatings have excellent waterproof and self-cleaning functions and can remain clean for a long time.
[0003] The technical development basis of the self-cleaning coating in the prior art is based on the principle of bionics, and most of the cleaning coatings designed based on the "lotus leaf self-cleaning principle" have achieved success;
[0004] For example, the Chinese patent with authorization announcement number CN101962514B discloses a long-durable super-hydrophobic self-cleaning coating and its preparation method. The coating material described in the invention is formed by curing and drying at room temperature with nanoparticles with photocatalytic activity, low surface free energy polymers and cross-linking agents, wherein the low surface free energy polymers are composed of one or more of fluorinated polysiloxanes, polydimethylsiloxanes and polymethylphenylsiloxanes containing active groups such as hydroxyalkoxy, carbon-carbon double bonds, silanol or silanoxy, etc. The cross-linking agent is hydrogen silicone oil or aminosilane, and the mass content of photocatalytic nanoparticles in the coating is between 10-60%. The coating is formed by self-organization of nanoparticles into micro-nano structures, and together with a cross-linked film-forming matrix with low surface energy, a super-hydrophobic self-cleaning coating with a lotus leaf effect is obtained, and the photocatalytic decomposition characteristics of nanoparticles on organic pollutants are used to achieve the durability of the lotus leaf-type super-hydrophobic characteristics of the coating, which is suitable for large-area construction, has good weather resistance, and has outstanding self-cleaning characteristics;
[0005] However, the main components of some current self-cleaning coatings are inorganic substances that provide a rough structure. However, inorganic nanoparticles often have a large specific surface area and high surface energy, and tend to agglomerate easily, resulting in reduced coating performance, reduced coating flatness, and surface defects such as cracks and bubbles. At the same time, inorganic nanoparticles have poor compatibility with resins and are prone to phase separation after mixing. As a result, the self-cleaning effect of the self-cleaning polyurethane thermal insulation coating material obtained is poor and the durability is not high. Summary of the invention
[0006] In order to improve the self-cleaning effect and durability of a self-cleaning polyurethane thermal insulation coating material, the present application provides a self-cleaning polyurethane thermal insulation coating material for application on a building surface and a preparation method thereof.
[0007] The self-cleaning polyurethane thermal insulation coating material for building surfaces provided in this application and the preparation method thereof adopt the following technical scheme:
[0008] The self-cleaning polyurethane thermal insulation coating material for building surfaces and its preparation method include the following raw materials: oligomer diol, aromatic diisocyanate, organic solvent, catalyst, modified organosilicon oligomer, modified nano titanium dioxide particle solution; the molar ratio of the oligomer diol to the aromatic diisocyanate is 1:(3-5), and the mass ratio of the oligomer diol to the modified organosilicon oligomer and the modified nano titanium dioxide particle solution is 1:(1-3):(1-1.5).
[0009] By adopting the above technical scheme, modified silicone oligomers are added to the preparation of polyurethane coatings, which can improve the high temperature resistance, weather resistance and other properties of the polyurethane coatings and improve the durability of the coatings on the one hand, and the modified silicone oligomers can increase the surface energy of the composite coatings on the other hand, thereby improving the hydrophobicity of the polyurethane coatings; and then by compounding the modified nano titanium dioxide particle solution, the electrons in the valence band of the photocatalytic material nano titanium dioxide will be excited to jump to the conduction band under the action of light, leaving relatively stable holes on the valence band, and the defects and dangling bonds in the nano material will capture electrons or holes to diffuse them to the surface of the particles respectively, generating a strong redox potential, degrading organic matter into gas and water without consuming nano titanium dioxide, thereby removing surface organic pollutants; and the modified nano titanium dioxide particle solution can generate crosslinking with the modified silicone oligomer and polyurethane, thereby improving the compatibility between the nano particles and the resin, and at the same time, the particles are wrapped by a large number of oligomers to improve the roughness, thereby effectively improving the hydrophobicity of the coating.
[0010] Preferably, the oligomer diol is one of polypropylene glycol and polytetramethylene ether glycol.
[0011] Preferably, the aromatic diisocyanate is one of diphenylmethane diisocyanate and toluene diisocyanate.
[0012] The organic solvent is propylene glycol; the catalyst is dibutyltin dilaurate; the solid-liquid ratio of the oligomer diol to the organic solvent is 1:(10-13) g / mL; the mass ratio of the oligomer diol to the catalyst is 1:(0.014-0.09)
[0013] Preferably, the modified organosilicon oligomer raw material includes alkaline organosilicon oligomer, anhydrous ethanol, and perfluorodecyltrimethylsilane in a mass ratio of 1:(0.4-0.6):(0.08-0.1).
[0014] By adopting the above technical scheme, the alkaline silicone oligomer is modified with perfluorodecyltrimethylsilane. Perfluorodecyltrimethylsilane has a very high surface tension, so it can improve the anti-adhesion property of the coating surface, prevent the adhesion of pollutants, and make the surface easier to clean; at the same time, it can also enhance the weather resistance and chemical resistance of the coating surface, making the coating more durable.
[0015] Preferably, the alkaline organosilicon oligomer is composed of the following raw materials in parts by weight: 30-36 parts of anhydrous ethanol, 3-5 parts of deionized water, 1-3 parts of aqueous ammonia, 0.4-0.6 parts of silane coupling agent KH-560, and 3.5-5.5 parts of tetraethyl orthosilicate.
[0016] Preferably, the raw materials of the modified nano-titanium dioxide particle solution include nano-titanium dioxide particle solution, anhydrous ethanol, and perfluorodecyltrimethylsilane in a mass ratio of 1:(0.5-0.7):(0.08-0.1).
[0017] By adopting the above technical scheme, the nano titanium dioxide particle solution is modified by using perfluorodecyltrimethylsilane, so that a silicone modified layer can be formed on the surface of the nano titanium dioxide, thereby improving the hydrophobicity of the surface, thereby improving the dispersibility of the nano titanium dioxide in the solution, making it more evenly dispersed in the coating, and improving the self-cleaning effect of the coating. At the same time, the modified nano titanium dioxide particles can be cross-linked with the modified silicone oligomer and polyurethane, thereby improving the compatibility between the nano particles and the resin, thereby further improving the durability of the coating.
[0018] Preferably, the nano titanium dioxide particle solution is composed of the following raw materials in parts by weight: 30-40 parts of anhydrous ethanol, 3-5 parts of deionized water, 0.9-1.3 parts of ammonia water, and 2-2.5 parts of tetrabutyl titanate.
[0019] The present application also provides a method for preparing a self-cleaning polyurethane thermal insulation coating material for building surface application, comprising the following steps:
[0020] After adding the oligomer diol into the reactor, heat it to 110-120°C and evacuate until there are no bubbles in the reactor, then cool it to 70-80°C, add an organic solvent and a catalyst into the reactor, and stir and reflux for 8-18 minutes; add an aromatic diisocyanate and react for 2-4 hours; add a modified organosilicon oligomer and react for 1-2 hours, then add a modified nano titanium dioxide particle solution, continue stirring for 15-25 minutes, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0021] Preferably, the method for preparing the modified organosilicon oligomer comprises the following steps:
[0022] S1. Take 30-36 parts of anhydrous ethanol, add 3-5 parts of deionized water and mix well, then add 1-3 parts of ammonia water and 0.4-0.6 parts of silane coupling agent KH-560 respectively, stir for 5-10 minutes to obtain a mixture; add 3.5-5.5 parts of tetraethyl orthosilicate dropwise into the mixture under stirring, continue stirring for 1-2 hours to obtain a basic organosilicon oligomer;
[0023] S2. Dilute the alkaline silicone oligomer obtained in S1 with anhydrous ethanol in a mass ratio of 1:(0.4-0.6), then add perfluorodecyltrimethylsilane dropwise, the weight ratio of perfluorodecyltrimethylsilane to the alkaline oligomer is (0.08-0.1):1, stir at room temperature for 10-20 minutes to obtain a modified silicone oligomer.
[0024] Preferably, the method for preparing the modified nano titanium dioxide particle solution comprises the following steps:
[0025] S1. Measure 30-40 parts of anhydrous ethanol, add 3-5 parts of deionized water, 0.9-1.3 parts of ammonia water, and stir to obtain a mixture; add 2-2.5 parts of tetrabutyl titanate dropwise to the mixture under stirring, and stir at 60-70 ° C for 6-8h to obtain a nano titanium dioxide particle solution;
[0026] S2. Dilute the nano-titanium dioxide particle solution with anhydrous ethanol in a mass ratio of 1:(0.5-0.7), then add perfluorodecyltrimethylsilane dropwise, the weight ratio of perfluorodecyltrimethylsilane to alkaline oligomer is (0.08-0.1):1, stir at room temperature for 10-20 minutes to obtain a modified nano-titanium dioxide particle solution.
[0027] In summary, the present application includes at least one of the following beneficial technical effects:
[0028] 1. By adopting the above technical scheme, a modified silicone oligomer is added to the preparation of the polyurethane coating, which can improve the high temperature resistance, weather resistance and other properties of the polyurethane coating and improve the durability of the coating. On the other hand, the modified silicone oligomer can increase the surface energy of the composite coating, thereby improving the hydrophobicity of the polyurethane coating;
[0029] 2. Then, by compounding the modified nano titanium dioxide particle solution, the photocatalytic material nano titanium dioxide will be excited to jump from the valence band to the conduction band under the action of light, leaving relatively stable holes in the valence band. The defects and dangling bonds in the nanomaterial will capture electrons or holes and diffuse them to the surface of the particles respectively, generating a strong redox potential, degrading organic matter into gas and water without consuming nano titanium dioxide, thereby removing surface organic pollutants; and the modified nano titanium dioxide particle solution can be cross-linked with modified silicone oligomers and polyurethanes, thereby improving the compatibility between the nanoparticles and the resin. At the same time, the particles are wrapped by a large number of oligomers to improve the roughness, thereby effectively improving the hydrophobicity of the coating. DETAILED DESCRIPTION
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] Preparation Example
[0032] Preparation Example 1 Preparation of modified silicone oligomer
[0033] Preparation Example 1.1
[0034] S1. Take 30g of anhydrous ethanol, add 3g of deionized water and mix well, then add 1g of ammonia water and 0.4g of silane coupling agent KH-560 respectively, stir at room temperature and stirring speed of 400rpm for 5min to obtain a mixture; add 3.5g of tetraethyl orthosilicate dropwise into the mixture under stirring, continue stirring at room temperature and stirring speed of 400rpm for 1h to obtain a basic organosilicon oligomer;
[0035] S2. 10 g of the alkaline organosilicon oligomer obtained in S1 was mixed and diluted with 4 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and stirred at room temperature at a stirring speed of 600 rpm for 10 min to obtain a modified organosilicon oligomer.
[0036] Preparation Example 1.2
[0037] S1. Take 33g of anhydrous ethanol, add 4g of deionized water and mix well, then add 2g of ammonia water and 0.5g of silane coupling agent KH-560 respectively, stir at room temperature and stirring speed of 450rpm for 8min to obtain a mixture; add 4.5g of tetraethyl orthosilicate dropwise into the mixture under stirring, continue stirring at room temperature and stirring speed of 450rpm for 1.5h to obtain a basic organosilicon oligomer;
[0038] S2. 10 g of the alkaline organosilicon oligomer obtained in S1 was mixed and diluted with 4 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and stirred at room temperature at a stirring speed of 650 rpm for 15 min to obtain a modified organosilicon oligomer.
[0039] Preparation Example 1.3
[0040] S1. Take 36g of anhydrous ethanol, add 5g of deionized water and mix well, then add 3g of ammonia water and 0.6g of silane coupling agent KH-560 respectively, stir at room temperature and stirring speed of 500rpm for 10min to obtain a mixture; add 5.5g of tetraethyl orthosilicate dropwise into the mixture under stirring, continue stirring at room temperature and stirring speed of 500rpm for 2h to obtain a basic organosilicon oligomer;
[0041] S2. 10 g of the alkaline organosilicon oligomer obtained in S1 was mixed and diluted with 4 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and stirred at room temperature at a stirring speed of 700 rpm for 20 min to obtain a modified organosilicon oligomer.
[0042] Preparation Example 1.4
[0043] The difference between Preparation Example 1.4 and Preparation Example 1.1 is that in Preparation Example 1.4, the mass of the basic organosilicon oligomer used in step S2 is 10 g, the mass of anhydrous ethanol is 5 g, and the mass of 1% perfluorodecyltrimethylsilane is 0.9 g.
[0044] Preparation Example 1.5
[0045] The difference between Preparation Example 1.5 and Preparation Example 1.1 is that in Preparation Example 1.5, the mass of the basic organosilicon oligomer used in step S2 is 10 g, the mass of anhydrous ethanol is 6 g, and the mass of 1% perfluorodecyltrimethylsilane is 1 g.
[0046] Preparation Example 1.6
[0047] The difference between Preparation Example 1.6 and Preparation Example 1.1 is that in Preparation Example 1.6, the mass of the basic organosilicon oligomer used in step S2 is 10 g, the mass of anhydrous ethanol is 2 g, and the mass of 1% perfluorodecyltrimethylsilane is 0.6 g.
[0048] Preparation Example 1.7
[0049] The difference between Preparation Example 1.7 and Preparation Example 1.1 is that in Preparation Example 1.7, the mass of the basic organosilicon oligomer used in step S2 is 10 g, the mass of anhydrous ethanol is 8 g, and the mass of 1% perfluorodecyltrimethylsilane is 1.2 g.
[0050] Preparation Example 2 Preparation of modified nano titanium dioxide particle solution
[0051] Preparation Example 2.1
[0052] S1. 30 g of anhydrous ethanol was measured, 3 g of deionized water and 0.9 g of ammonia water were added in sequence, and the mixture was stirred at 60 ° C and 400 rpm for 10 min to obtain a mixture; 2 g of tetrabutyl titanate was added dropwise to the mixture under stirring, and stirred at 60 ° C for 6 h to obtain a nano-titanium dioxide particle solution;
[0053] S2. 10 g of the nano-titanium dioxide particle solution obtained in S1 was mixed and diluted with 5 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and the mixture was stirred at room temperature at a stirring speed of 600 rpm for 10 min to obtain a modified nano-titanium dioxide particle solution.
[0054] Preparation Example 2.2
[0055] S1. 35 g of anhydrous ethanol was measured, 4 g of deionized water and 1.1 g of ammonia water were added in sequence, and the mixture was stirred at 65 ° C and 450 rpm for 15 min to obtain a mixture; 2.3 g of tetrabutyl titanate was added dropwise to the mixture under stirring, and stirred at 65 ° C for 7 h to obtain a nano-titanium dioxide particle solution;
[0056] S2. 10 g of the nano-titanium dioxide particle solution obtained in S1 was mixed and diluted with 5 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and stirred at room temperature at a stirring speed of 650 rpm for 15 min to obtain a modified nano-titanium dioxide particle solution.
[0057] Preparation Example 2.3
[0058] S1. 40 g of anhydrous ethanol was measured, 5 g of deionized water and 1.3 g of ammonia water were added in sequence, and the mixture was stirred at 70 ° C and 500 rpm for 20 min to obtain a mixture; 2.5 g of tetrabutyl titanate was added dropwise to the mixture under stirring, and stirred at 70 ° C for 8 h to obtain a nano-titanium dioxide particle solution;
[0059] S2. 10 g of the nano-titanium dioxide particle solution obtained in S1 was mixed and diluted with 5 g of anhydrous ethanol, and then 0.8 g of 1% perfluorodecyltrimethylsilane was added dropwise, and the mixture was stirred at room temperature at a stirring speed of 700 rpm for 20 min to obtain a modified nano-titanium dioxide particle solution.
[0060] Preparation Example 2.4
[0061] The difference between Preparation Example 2.4 and Preparation Example 2.1 is that in Preparation Example 2.4, the mass of the nano-titanium dioxide particle solution used in step S2 is 10 g, the mass of anhydrous ethanol is 6 g, and the mass of 1% perfluorodecyltrimethylsilane is 0.9 g.
[0062] Preparation Example 2.5
[0063] The difference between Preparation Example 2.5 and Preparation Example 2.1 is that in Preparation Example 2.5, the mass of the nano-titanium dioxide particle solution used in step S2 is 10 g, the mass of anhydrous ethanol is 7 g, and the mass of 1% perfluorodecyltrimethylsilane is 1 g.
[0064] Preparation Example 2.6
[0065] The difference between Preparation Example 2.6 and Preparation Example 2.1 is that in Preparation Example 2.6, the mass of the nano-titanium dioxide particle solution used in step S2 is 10 g, the mass of anhydrous ethanol is 4 g, and the mass of 1% perfluorodecyltrimethylsilane is 0.6 g.
[0066] Preparation Example 2.7
[0067] The difference between Preparation Example 2.7 and Preparation Example 2.1 is that in Preparation Example 2.7, the mass of the nano-titanium dioxide particle solution used in step S2 is 10 g, the mass of anhydrous ethanol is 9 g, and the mass of 1% perfluorodecyltrimethylsilane is 1.2 g.
[0068] Example
[0069] Example 1
[0070] After adding 10g of polytetramethylene ether glycol (molecular weight 650) into the reactor, heat to 110°C and evacuate until there are no bubbles in the reactor, cool to 70°C, add 100mL of organic solvent propylene glycol and 0.22g of catalyst dibutyltin dilaurate into the reactor, stir and reflux for 8min; add 11.55g of diphenylmethane diisocyanate and react for 2h; add 10g of the modified silicone oligomer prepared in Preparation Example 1.1 and react for 1h, then add 10g of the modified nano titanium dioxide particle solution prepared in Preparation Example 2.1, continue stirring for 15min, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0071] Example 2
[0072] After adding 10g of polytetramethylene ether glycol into the reactor, heat it to 115°C and evacuate until there are no bubbles in the reactor, cool it to 75°C, add 110mL of organic solvent propylene glycol and 0.5g of catalyst dibutyltin dilaurate into the reactor, stir and reflux for 13min; add 15.4g of diphenylmethane diisocyanate and react for 3h; add 10g of the modified silicone oligomer prepared in Preparation Example 1.1 and react for 1.5h, then add 10g of the modified nano titanium dioxide particle solution prepared in Preparation Example 2.1, continue stirring for 20min, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0073] Example 3
[0074] After adding 10g of polytetramethylene ether glycol into the reactor, heat it to 120°C and evacuate until there are no bubbles in the reactor, cool it to 80°C, add 130mL of organic solvent propylene glycol and 0.9g of catalyst dibutyltin dilaurate into the reactor, stir and reflux for 18min; add 19.25g of diphenylmethane diisocyanate and react for 4h; add 10g of the modified silicone oligomer prepared in Preparation Example 1.1 and react for 2h, then add 10g of the modified nano titanium dioxide particle solution prepared in Preparation Example 2.1, continue stirring for 25min, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0075] Example 4
[0076] After adding 10g of polypropylene glycol (molecular weight 2000) into the reactor, heat it to 110°C and evacuate until there are no bubbles in the reactor, cool it to 70°C, add 100mL of organic solvent propylene glycol and 0.14g of catalyst dibutyltin dilaurate into the reactor, stir and reflux for 8min; add 3.75g of diphenylmethane diisocyanate and react for 2h; add 10g of the modified silicone oligomer prepared in Preparation Example 1.1 and react for 1h, then add 10g of the modified nano titanium dioxide particle solution prepared in Preparation Example 2.1, continue stirring for 15min, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0077] Example 5
[0078] After adding 10g of polytetramethylene ether glycol (molecular weight 650) into the reactor, heat it to 110°C and evacuate until there are no bubbles in the reactor, cool it to 70°C, add 100mL of organic solvent propylene glycol and 0.18g of catalyst dibutyltin dilaurate into the reactor, stir and reflux for 8min; add 8g of toluene diisocyanate and react for 2h; add 10g of the modified silicone oligomer prepared in Preparation Example 1.1 and react for 1h, then add 10g of the modified nano titanium dioxide particle solution prepared in Preparation Example 2.1, continue stirring for 15min, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
[0079] Example 6
[0080] The difference between Example 6 and Example 1 is that the modified organosilicon oligomer used in Example 6 comes from Preparation Example 1.1, with a mass of 20 g; and the modified nano-titanium dioxide particle solution comes from Preparation Example 2.1, with a mass of 12.5 g.
[0081] Example 7
[0082] The difference between Example 7 and Example 1 is that the modified organosilicon oligomer used in Example 7 comes from Preparation Example 1.1, with a mass of 30 g; and the modified nano-titanium dioxide particle solution comes from Preparation Example 2.1, with a mass of 15 g.
[0083] Example 8
[0084] The difference between Example 8 and Example 1 is that the modified organosilicon oligomer used in Example 8 comes from Preparation Example 1.2, with a mass of 10 g.
[0085] Example 9
[0086] The difference between Example 9 and Example 1 is that the modified organosilicon oligomer used in Example 9 comes from Preparation Example 1.3, with a mass of 10 g.
[0087] Example 10
[0088] The difference between Example 10 and Example 1 is that the modified organosilicon oligomer used in Example 10 comes from Preparation Example 1.4, with a mass of 10 g.
[0089] Embodiment 11
[0090] The difference between Example 11 and Example 1 is that the modified organosilicon oligomer used in Example 11 comes from Preparation Example 1.5, with a mass of 10 g.
[0091] Example 12
[0092] The difference between Example 12 and Example 1 is that the modified organosilicon oligomer used in Example 12 comes from Preparation Example 1.6, with a mass of 10 g.
[0093] Embodiment 13
[0094] The difference between Example 13 and Example 1 is that the modified organosilicon oligomer used in Example 13 comes from Preparation Example 1.7, with a mass of 10 g.
[0095] Embodiment 14
[0096] The difference between Example 14 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 14 comes from Preparation Example 2.2, with a mass of 10 g.
[0097] Embodiment 15
[0098] The difference between Example 15 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 15 comes from Preparation Example 2.3, with a mass of 10 g.
[0099] Example 16
[0100] The difference between Example 16 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 16 comes from Preparation Example 2.4, with a mass of 10 g.
[0101] Embodiment 17
[0102] The difference between Example 17 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 17 comes from Preparation Example 2.5, with a mass of 10 g.
[0103] Embodiment 18
[0104] The difference between Example 18 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 18 comes from Preparation Example 2.6, with a mass of 10 g.
[0105] Embodiment 19
[0106] The difference between Example 19 and Example 1 is that the modified nano-titanium dioxide particle solution used in Example 19 comes from Preparation Example 2.7, with a mass of 10 g.
[0107] Comparative Example
[0108] Comparative Example 1
[0109] The difference between Comparative Example 1 and Example 1 is that the modified organosilicon oligomer used in Comparative Example 1 comes from Preparation Example 1.1, with a mass of 5 g; and the modified nano-titanium dioxide particle solution comes from Preparation Example 2.1, with a mass of 5 g.
[0110] Comparative Example 2
[0111] The difference between Comparative Example 2 and Example 1 is that the modified organosilicon oligomer used in Comparative Example 2 comes from Preparation Example 1.1, with a mass of 40 g; and the modified nano-titanium dioxide particle solution comes from Preparation Example 2.1, with a mass of 20 g.
[0112] Performance testing
[0113] 1. The water contact angles of the self-cleaning polyurethane thermal insulation coating materials for building surfaces obtained in Examples 1-19 and Comparative Examples 1-2 were tested using GB / T 30693-2014 “Measurement of the contact angle of plastic film with water”. The results are shown in Table 1.
[0114] Table 1 Water contact angle test results
[0115]
[0116]
[0117] It can be seen from the test results in Table 1 that the water contact angle of the self-cleaning polyurethane thermal insulation coating material applied to the building surface provided by the present application can reach more than 150°, indicating that the self-cleaning polyurethane thermal insulation coating material provided by the present application has super hydrophobicity and has self-cleaning ability similar to the surface of a lotus leaf.
[0118] It can be seen from the test results of Comparative Examples 1-2 that when the mass ratio of the oligomer diol to the modified silicone oligomer and the modified nano-titanium dioxide particle solution used in the preparation of the self-cleaning polyurethane thermal insulation coating material for building surfaces in the present application is lower than or exceeds the range of 1:1-3:1-1.5, the water contact angle of the obtained polyurethane thermal insulation coating material is lower than 150°, that is, the obtained coating does not have super hydrophobicity.
[0119] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A self-cleaning polyurethane thermal insulation coating material for building surfaces, characterized by: Including the following ingredients: Oligomeric diol, aromatic diisocyanate, organic solvent, catalyst, modified organosilicon oligomer, modified nano-titanium dioxide particle solution; the molar ratio of the oligomeric diol to the aromatic diisocyanate is 1:(3-5), and the mass ratio of the oligomeric diol to the modified organosilicon oligomer and the modified nano-titanium dioxide particle solution is 1:(1-3):(1-1.5).
2. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 1, characterized in that: The oligomer diol is one of polypropylene glycol and polytetramethylene ether glycol; the aromatic diisocyanate is one of diphenylmethane diisocyanate and toluene diisocyanate.
3. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 1, characterized in that: The organic solvent is propylene glycol; the catalyst is dibutyltin dilaurate; the solid-liquid ratio of the oligomer diol to the organic solvent is 1:(10-13) g / mL; the mass ratio of the oligomer diol to the catalyst is 1:(0.014-0.09).
4. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 1, characterized in that: The modified organic silicon oligomer raw material comprises alkaline organic silicon oligomer, anhydrous ethanol and perfluorodecyltrimethylsilane in a mass ratio of 1:(0.4-0.6):(0.08-0.1).
5. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 4, characterized in that: The alkaline organosilicon oligomer is composed of the following raw materials in parts by weight: 30-36 parts of anhydrous ethanol, 3-5 parts of deionized water, 1-3 parts of ammonia water, 0.4-0.6 parts of silane coupling agent KH-560, and 3.5-5.5 parts of tetraethyl orthosilicate.
6. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 1, characterized in that: The modified nano titanium dioxide particle solution raw materials include nano titanium dioxide particle solution, anhydrous ethanol, and perfluorodecyltrimethylsilane, and the mass ratio is 1: (0.5-0.7): (0.08-0.1).
7. The self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 6, characterized in that: The nano titanium dioxide particle solution is composed of the following raw materials in parts by weight: 30-40 parts of anhydrous ethanol, 3-5 parts of deionized water, 0.9-1.3 parts of ammonia water, and 2-2.5 parts of tetrabutyl titanate.
8. The method for preparing the self-cleaning polyurethane thermal insulation coating material for building surface application according to any one of claims 1 to 7, characterized in that: The following steps are involved: After adding the oligomer diol into the reactor, heat it to 110-120°C and evacuate until there are no bubbles in the reactor, then cool it to 70-80°C, add an organic solvent and a catalyst into the reactor, and stir and reflux for 8-18 minutes; add an aromatic diisocyanate and react for 2-4 hours; add a modified organosilicon oligomer and react for 1-2 hours, then add a modified nano titanium dioxide particle solution, continue stirring for 15-25 minutes, and cool to room temperature to obtain a self-cleaning polyurethane thermal insulation coating material for building surfaces.
9. The method for preparing the self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 8, characterized in that: The method for preparing the modified organosilicon oligomer comprises the following steps: S1. Take 30-36 parts of anhydrous ethanol, add 3-5 parts of deionized water and mix well, then add 1-3 parts of ammonia water and 0.4-0.6 parts of silane coupling agent KH-560 respectively, stir for 5-10 minutes to obtain a mixture; add 3.5-5.5 parts of tetraethyl orthosilicate dropwise into the mixture under stirring, continue stirring for 1-2 hours to obtain a basic organosilicon oligomer; S2. Dilute the alkaline silicone oligomer obtained in S1 with anhydrous ethanol in a mass ratio of 1:(0.4-0.6), then add perfluorodecyltrimethylsilane dropwise, the weight ratio of perfluorodecyltrimethylsilane to the alkaline oligomer is (0.08-0.1):1, stir at room temperature for 10-20 minutes to obtain a modified silicone oligomer.
10. The method for preparing the self-cleaning polyurethane thermal insulation coating material for building surface application according to claim 8, characterized in that: The method for preparing the modified nano titanium dioxide particle solution comprises the following steps: S1. Measure 30-40 parts of anhydrous ethanol, add 3-5 parts of deionized water, 0.9-1.3 parts of ammonia water, and stir to obtain a mixture; add 2-2.5 parts of tetrabutyl titanate dropwise to the mixture under stirring, and stir at 60-70 ° C for 6-8h to obtain a nano titanium dioxide particle solution; S2. Dilute the nano-titanium dioxide particle solution with anhydrous ethanol in a mass ratio of 1:(0.5-0.7), then add perfluorodecyltrimethylsilane dropwise, the weight ratio of perfluorodecyltrimethylsilane to alkaline oligomer is (0.08-0.1):1, stir at room temperature for 10-20 minutes to obtain a modified nano-titanium dioxide particle solution.
Citation Information
Patent Citations
Aluminum alloy door / window flame-retardant antibacterial coating
CN106118372A
Processing and use of particulate materials, especially for preparing waterborne paint compositions
EP0837111A1
Cited By
Reflection heat insulation and heat preservation double-effect integrated aerogel heat insulation finish paint and preparation method thereof
CN119931391A
Reflective heat-insulating and heat-preserving aerogel paint and preparation method thereof
CN119931391B