Active agent for surface pretreatment and preparation method thereof
By modifying the combination of polyurethane acrylate, adhesion accelerator and photoinitiator, the adhesion between metal or plastic substrate and UV coatings is improved, the problems of insufficient adhesion and poor impact resistance are solved, and air pollution is reduced. Optimized coating performance.
Patent Information
- Application Number
- CN202411078342.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, insufficient adhesion between metal or plastic substrate and coating leads to poor impact resistance of the coating and air pollution problems caused by chromatic aberration and sandblasting operations.
Modified polyurethane acrylate is used as the resin main body, combined with adhesion accelerator, coupling agent and photoinitiator, to enhance the adhesion of UV coatings to metal or plastic substrates through polymerization, and to introduce cellulose into the polyurethane acrylate segment. Whiskers increase surface roughness and strength and improve the impact resistance of the coating.
It significantly improves the adhesion between metal or plastic substrates and UV coatings and the impact resistance of the coating, solves the problems of insufficient adhesion and chromatic aberration, and reduces air pollution caused by sandblasting operations.
Smart Images

Figure BDA0004983002430000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface treatment agents, and in particular to an active agent for surface pretreatment and a preparation method thereof. Background Art
[0002] In the chemical industry, it is often necessary to color metal and plastic products to make the products have a better appearance and enhance their appeal to customers. Among the methods of coloring metals, the electrolytic coloring method is to form a dense oxide film by anodizing the aluminum plate, and then reduce and deposit the metal ions through electrolytic reaction under specific conditions to form color. However, since the electrolytic coloring method relies on electrolysis to form color, scratches often appear on the surface of the aluminum material, which is difficult to repair. In addition, the color of the anodized aluminum material will differ due to the type, concentration, activation time, and temperature of the electrolyte and the activator. Therefore, the anodized aluminum materials produced at different times and in different factories are prone to color differences. The method of coloring with paint can be used for plastic and metal products, but in order to improve the adhesion of the paint to the metal or plastic, it is often necessary to perform sandblasting before applying the paint. However, sandblasting is prone to cause air pollution. In addition, when the substrate is plastic, there is a problem that the plastic is not resistant to high temperatures and is not easy to sandblast. Therefore, surface treatment activators that can improve surface adhesion have gradually entered everyone's field of vision.
[0003] Patent CN113480571A discloses a photosensitive phytic acid-based adhesion promoter, a preparation method and an application thereof. A phytic acid aqueous solution is mixed with glycidyl methacrylate, reacted under the action of a phase transfer catalyst and an inhibitor, and a photosensitive phytic acid is obtained after purification. The photosensitive phytic acid not only has metal chelating ability, but can also react with hydroxyl groups on the metal surface, thereby improving the adhesion between the coating and the substrate. However, this adhesion promoter may corrode the metal surface, allowing water vapor to easily enter the gap and accelerate the corrosion of the metal.
[0004] Patent CN104440923B discloses a radiation-curing coating adhesion promoter and a preparation method thereof. The adhesion promoter has a linear structure, one end of the molecular structure has a (meth)acrylate double bond, the other end is a carboxyl structure, and the middle skeleton segment is a poly-ε-caprolactone molecular structure. The skeleton structure segment of poly-ε-caprolactone is added to the molecular structure of the conventional adhesion promoter, which solves the problem of poor coating fastness caused by the conventional adhesion promoter due to short segments, large curing shrinkage, poor flexibility, etc. However, the increase in the molecular weight of the adhesion promoter may reduce the density of the carboxyl group and thus reduce the fastness of the coating. This method still has room for improvement.
[0005] Therefore, there is an urgent need in the market for a surface pretreatment active agent that can improve the adhesion between a metal or plastic substrate and a coating. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to obtain a surface pretreatment active agent that can enhance the impact resistance of the coating and improve the adhesion between the metal or plastic substrate and the UV coating.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On one hand, the present invention provides an active agent for surface pretreatment, which comprises the following raw materials in parts by weight: 30-50 parts of modified polyurethane acrylate, 4-6 parts of adhesion promoter, 1-2 parts of coupling agent, and 1-2 parts of photoinitiator.
[0009] This application uses modified polyurethane acrylate as the main resin, and uses adhesion promoter, coupling agent and photoinitiator as additives to prepare a surface pretreatment active agent that can improve the bonding effect between metal or plastic substrates and UV coatings. During the photocuring process, the UV coating can undergo a polymerization reaction with the double bonds in the surface pretreatment active agent to enhance the adhesion between the two and improve the impact resistance of the coating.
[0010] In some embodiments, the method for preparing the modified polyurethane acrylate comprises the following steps:
[0011] S1. Add cellulose whiskers and acetone into a reaction vessel, stir for 20-30 minutes, add isophorone diisocyanate, heat to 70-80°C and react for 1-2 hours, cool to room temperature, add isoamyl alcohol for precipitation, wash, filter and dry the precipitate to obtain modified cellulose whiskers;
[0012] S2, adding isophorone diisocyanate, polytetramethylene glycol, the modified cellulose whisker obtained in step S1 and a catalyst into a reaction container, reacting at 70-80° C. for 1-2 hours, cooling to 50-60° C., adding a chain extender, continuing the reaction for 0.5-1 hour, adding pentaerythritol triacrylate, and reacting for 1-2 hours to obtain modified polyurethane acrylate.
[0013] Preferably, the preparation method of the modified polyurethane acrylate comprises the following steps:
[0014] S1, adding cellulose whiskers and acetone into a reaction vessel, stirring for 20-30 minutes, adding isophorone diisocyanate, heating to 70-80°C and reacting for 1-2 hours, wherein the mass ratio of cellulose whiskers to isophorone diisocyanate is (0.3-0.5):1, cooling to room temperature, adding isoamyl alcohol for precipitation, washing, filtering and drying the precipitate to obtain modified cellulose whiskers;
[0015] S2, adding isophorone diisocyanate, polytetrahydrofuran diol, the modified cellulose whisker obtained in step S1 and tetraisopropyl titanate into a reaction container, wherein the mass ratio of isophorone diisocyanate to polytetrahydrofuran diol is 1:(1-2), reacting at 70-80° C. for 1-2 h, cooling to 50-60° C., adding 1,4-butanediol, continuing the reaction for 0.5-1 h, adding pentaerythritol triacrylate, and reacting for 1-2 h to obtain modified polyurethane acrylate.
[0016] The present application uses isophorone diisocyanate to modify cellulose whiskers to improve the activity of cellulose whiskers, and improve the grafting rate and compatibility of cellulose whiskers on polyurethane acrylate. Cellulose whiskers are introduced into the polyurethane acrylate chain segment, which, on the one hand, increases the roughness of the metal or plastic surface when used on the metal or plastic surface, and on the other hand, enhances the strength and toughness of the polyurethane acrylate, making the surface pretreatment active agent less likely to be destroyed, which is beneficial to improving the impact resistance of the coating.
[0017] In some embodiments, the cellulose whiskers have a length of 100-500 nm.
[0018] In some embodiments, the mass ratio of the modified cellulose whiskers to the chain extender is (0.6-0.7):1.
[0019] The present application can make the surface pretreatment active agent have a better pretreatment effect by selecting a specific ratio of modified cellulose whiskers and chain extenders and limiting the length of the cellulose whiskers, thereby improving the adhesion between the plastic or metal and the coating. This may be because the residual modified cellulose in the system can be randomly arranged in the polyurethane acrylate and is more likely to be exposed on the surface of the polyurethane acrylate, thereby increasing the roughness of the surface of the plastic or metal and the coating.
[0020] In some embodiments, the filler is one or more of titanium dioxide, calcium carbonate, and barium sulfate.
[0021] Preferably, the filler is titanium dioxide.
[0022] In some embodiments, the method for preparing the adhesion promoter comprises the following steps:
[0023] A1. Add hydroxyethyl methacrylate, gluconolactone and stannous octoate into a reaction vessel, and stir at 150-170° C. for 3-6 hours to obtain polygluconolactone containing double bonds;
[0024] A2. Add the double-bond polygluconolactone obtained in step A1 and phosphoric acid into a reaction vessel, heat to 70-80° C., and react for 2-4 hours to obtain an adhesion promoter.
[0025] The present application uses hydroxyethyl methacrylate and glucono-lactone to synthesize a compound containing a long-chain structure with terminal double bonds and multiple hydroxyl groups. The presence of the double bond can enable the adhesion promoter to react with the UV coating to enhance the adhesion of the coating to the plastic or metal, and the multiple hydroxyl groups make the double-bonded polyglucono-lactone have a high reactivity with phosphoric acid, ensuring that one molecule of double-bonded polyglucono-lactone can react with at least two phosphoric acids, so that two phosphate groups are formed on the adhesion promoter, which is beneficial to improving the adhesion of the surface pretreatment active agent to the metal.
[0026] In some embodiments, the adhesion promoter has a number average molecular weight of 400-700.
[0027] The present application controls the number average molecular weight to make the length of the constructed chain segment appropriate, which can not only solve the problem of poor coating fastness caused by conventional adhesion promoters due to short chain segments, large curing shrinkage, poor flexibility, etc., but also solve the problem of low content of phosphate groups attached to the chain segments due to the adhesion promoter being too long, thereby reducing the adhesion between the surface pretreatment active agent and the metal.
[0028] In some embodiments, the mass ratio of hydroxyethyl methacrylate to gluconolactone is 1:(2.5-3.5).
[0029] The present application can make the adhesion of the coating higher by selecting a specific ratio of hydroxyethyl methacrylate and gluconolide. This may be because the residual gluconolide contains multiple hydroxyl groups and has strong water absorption, which remains in the surface pretreatment surfactant and affects the adhesion of the coating.
[0030] In some embodiments, the mass ratio of the double-bond-containing polyglucoside lactone to phosphoric acid is 1:(0.6-0.7).
[0031] The present application can load multiple phosphate groups on the polyglucoside containing double bonds by selecting a specific ratio of polyglucoside containing double bonds and phosphoric acid, thereby improving the binding force between the adhesion promoter and the metal and improving the adhesion between the metal and the coating.
[0032] In some embodiments, the coupling agent is one or more of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.
[0033] Preferably, the coupling agent is a silane coupling agent.
[0034] Further preferably, the silane coupling agent is KH550.
[0035] In some embodiments, the photoinitiator is one or more of TPO, photoinitiator 2959, photoinitiator 184, photoinitiator 1173, and photoinitiator 651.
[0036] Preferably, the photoinitiator is TPO.
[0037] On the other hand, the present invention provides a method for preparing an active agent for surface pretreatment, comprising the following steps: mixing modified polyurethane acrylate, an adhesion promoter, a coupling agent, and a photoinitiator, and stirring at 25-30° C. for 20-30 minutes to obtain the active agent.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] (1) The present invention uses modified polyurethane acrylate as the main resin, and the surface pretreatment active agent prepared by using an adhesion promoter, a coupling agent, and a photoinitiator as additives can improve the bonding effect between the metal or plastic substrate and the UV coating. During the photocuring process, the UV coating can undergo a polymerization reaction with the double bonds in the surface pretreatment active agent to enhance the adhesion between the two and improve the impact resistance of the coating.
[0040] (2) The present invention introduces cellulose whiskers into the polyurethane acrylate chain segment. On the one hand, when the cellulose whiskers are used on metal or plastic surfaces, the roughness of the metal or plastic surface is increased, thereby improving the adhesion of the coating. On the other hand, the strength and toughness of the polyurethane acrylate are enhanced, thereby ensuring that the surface pretreatment active agent for the metal or plastic surface is not easily destroyed, thereby improving the impact resistance of the coating. Furthermore, by limiting the ratio of the modified cellulose whiskers and the chain extender, the modified cellulose remaining in the system can be randomly arranged in the polyurethane acrylate, making it easier to be exposed on the surface of the polyurethane acrylate, thereby further improving the adhesion between the coatings.
[0041] (3) The present invention uses hydroxyethyl methacrylate and polyglucono-lactone to synthesize a compound containing a long-chain structure with a terminal double bond and multiple hydroxyl groups. The construction of the long-chain structure improves the fastness of the adhesion promoter and the coating. The multiple hydroxyl groups give the double-bonded polyglucono-lactone reactivity with phosphoric acid, so that a phosphate group is formed on the adhesion promoter, which is beneficial to improving the binding force of the surface pretreatment active agent metal. DETAILED DESCRIPTION
[0042] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0043] In the following examples and comparative examples, except for modified polyurethane acrylate and adhesion promoter, the other compounds and related reagents used can be purchased from the market, among which the length of cellulose whiskers is 100-500nm, purchased from Zhongke Jinyan (Beijing) Technology Co., Ltd.; adhesion promoter-5 is UV system adhesion promoter 9050, purchased from Shandong Shoucheng Chemical Co., Ltd.
[0044] Preparation Example 1
[0045] The preparation method of modified polyurethane acrylate-1 comprises the following steps:
[0046] S1. Add 1 g of cellulose whiskers and 10 g of acetone into a reaction vessel, stir for 25 min, add 2.5 g of isophorone diisocyanate, heat to 75 °C and react for 1.5 h, cool to room temperature, add 10 g of isoamyl alcohol for precipitation, wash, filter and dry the precipitate to obtain modified cellulose whiskers;
[0047] S2. Add 10 g of isophorone diisocyanate, 15 g of polytetramethylene glycol, 1 g of modified cellulose whisker obtained in step S1 and 0.001 g of tetraisopropyl titanate into a reaction container, react at 75° C. for 1.5 h, cool to 55° C., add 1.5 g of 1,4-butanediol, continue to react for 0.5 h, then add 5 g of pentaerythritol triacrylate, and react for 1 h to obtain modified polyurethane acrylate-1.
[0048] Preparation Example 2
[0049] The preparation method of modified polyurethane acrylate-2 comprises the following steps:
[0050] S1. Add 1 g of cellulose whiskers and 10 g of acetone into a reaction vessel, stir for 25 min, add 2.5 g of isophorone diisocyanate, heat to 75 °C and react for 1.5 h, cool to room temperature, add 10 g of isoamyl alcohol for precipitation, wash, filter and dry the precipitate to obtain modified cellulose whiskers;
[0051] S2, add 10g of isophorone diisocyanate, 15g of polytetramethylene glycol, 0.5g of modified cellulose whisker obtained in step S1 and 0.001g of tetraisopropyl titanate into a reaction container, react at 75°C for 1.5h, cool to 55°C, add 1.5g of BDO, continue to react for 0.5h, then add 5g of pentaerythritol triacrylate, and react for 1h to obtain modified polyurethane acrylate-2.
[0052] Preparation Example 3
[0053] The preparation method of polyurethane acrylate is as follows: 10g of isophorone diisocyanate, 15g of polytetramethylene glycol and 0.001g of tetraisopropyl titanate are added into a reaction container, reacted at 75°C for 1.5h, cooled to 55°C, 1.5g of BDO is added, the reaction is continued for 0.5h, 5g of pentaerythritol triacrylate is added, and the polyurethane acrylate is obtained after reacting for 1h.
[0054] Preparation Example 4
[0055] The preparation method of adhesion promoter-1 comprises the following steps:
[0056] A1, add 10g hydroxyethyl methacrylate, 30g gluconolactone and 0.1g stannous octoate into a reaction vessel, stir at 160°C for 5h to obtain polygluconolactone containing double bonds;
[0057] A2. Add 30 g of the double-bond polygluconolactone obtained in step A1 and 19.5 g of phosphoric acid into a reaction container, heat to 75° C., and obtain an adhesion promoter-1 with a number average molecular weight of 550.
[0058] Preparation Example 5
[0059] The preparation method of adhesion promoter-2 comprises the following steps:
[0060] A1, add 10g hydroxyethyl methacrylate, 40g gluconolactone and 0.1g stannous octoate into a reaction vessel, stir at 160°C for 5h to obtain polygluconolactone containing double bonds;
[0061] A2. Add 30 g of the double-bond polygluconolactone obtained in step A1 and 19.5 g of phosphoric acid into a reaction container, heat to 75° C., and obtain an adhesion promoter-2 having a number average molecular weight of 550.
[0062] Preparation Example 6
[0063] The preparation method of adhesion promoter-3 comprises the following steps:
[0064] A1, add 10g hydroxyethyl methacrylate, 30g gluconolactone and 0.1g stannous octoate into a reaction vessel, stir at 160°C for 5h to obtain polygluconolactone containing double bonds;
[0065] A2. Add 30 g of the double-bond polygluconolactone obtained in step A1 and 15 g of phosphoric acid into a reaction container, heat to 75° C., and obtain an adhesion promoter-3 having a number average molecular weight of 550.
[0066] Preparation Example 7
[0067] The preparation method of adhesion promoter-4 comprises the following steps:
[0068] A1, add 10g hydroxyethyl methacrylate, 30g gluconolactone and 0.1g stannous octoate into a reaction vessel, stir at 160°C for 5h to obtain polygluconolactone containing double bonds;
[0069] A2. Add 30 g of the double-bond polygluconolactone obtained in step A1 and 19.5 g of phosphoric acid into a reaction container, heat to 75° C., and obtain an adhesion promoter-4 having a number average molecular weight of 800.
[0070] Example 1
[0071] A surface pretreatment active agent comprises the following raw materials, measured in parts by weight: 140 parts of modified polyurethane acrylate, 15 parts of adhesion promoter, 1.5 parts of KH550 and 1.5 parts of TPO.
[0072] The preparation method of the active agent for surface pretreatment in this embodiment comprises the following steps: mixing modified polyurethane acrylate-1, adhesion promoter-1, KH550 and TPO and stirring at 27° C. for 25 minutes to obtain the active agent.
[0073] Example 2
[0074] A surface pretreatment active agent comprises the following raw materials, measured in parts by weight: 130 parts of modified polyurethane acrylate, 14 parts of adhesion promoter, 1 part of KH550 and 1 part of TPO.
[0075] The preparation method of the active agent for surface pretreatment in this embodiment comprises the following steps: mixing modified polyurethane acrylate-1, adhesion promoter-1, KH550 and TPO and stirring at 25° C. for 30 minutes to obtain the active agent.
[0076] Example 3
[0077] A surface pretreatment active agent comprises the following raw materials, measured in parts by weight: 150 parts of modified polyurethane acrylate, 16 parts of adhesion promoter, 2 parts of KH550 and 2 parts of TPO.
[0078] The preparation method of the active agent for surface pretreatment in this embodiment comprises the following steps: mixing modified polyurethane acrylate-1, adhesion promoter-1, KH550 and TPO and stirring at 30° C. for 25 minutes to obtain the active agent.
[0079] Example 4
[0080] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of adhesion promoter-1 is replaced by adhesion promoter-2.
[0081] Example 5
[0082] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of adhesion promoter-1 is replaced by adhesion promoter-3.
[0083] Example 6
[0084] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of adhesion promoter-1 is replaced by adhesion promoter-4.
[0085] Example 7
[0086] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of adhesion promoter-1 is replaced by adhesion promoter-5.
[0087] Example 8
[0088] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyurethane acrylate-1 is replaced by modified polyurethane acrylate-2.
[0089] Comparative Example 1
[0090] A surface pretreatment active agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyurethane acrylate-1 is replaced by polyurethane acrylate.
[0091] Performance Testing
[0092] (1) Sample preparation
[0093] The surface of the aluminum plate was repeatedly wiped with acetone for 3 times to remove organic pollutants on the surface of the aluminum plate. A layer of the surface pretreatment active agent obtained in the above embodiments and comparative examples was applied on the aluminum plate using a film applicator, with a wet film thickness of 50 μm. After drying, a polyurethane resin coating purchased from Langfang Fuchen New Materials Co., Ltd. was applied on the aluminum plate using a film applicator, with a wet film thickness of 120 μm. The coating was leveled at 50°C for 30 minutes, and then exposed to the crawler F300S light curing machine for 5 times for curing. The conveyor speed was set to 5.4 m / min, and the total irradiation energy was 800 mJ / cm 2 , a photocured coating attached to the aluminum plate was obtained.
[0094] (2) Test method
[0095] According to GB / T 9286-1998, the surface pretreatment activator coated on the aluminum sheet and the light-cured coating attached to the aluminum plate were subjected to a cross-cut test to evaluate the adhesion between the surface pretreatment activator and the aluminum sheet, and between the coating and the aluminum sheet. The adhesion between the surface pretreatment activator and the aluminum sheet was recorded as adhesion 1, and the adhesion between the coating and the aluminum sheet was recorded as adhesion 2. In addition, the impact resistance of the light-cured coating attached to the aluminum plate was tested according to GB / T 1732-1993. The test results are shown in Table 1:
[0096] Table 1
[0097]
[0098]
[0099] It can be seen from the data in Table 1 that the surface pretreatment active agent in Examples 1-3 of the present invention can improve the adhesion of the surface pretreatment active agent and the coating after being applied on the substrate, so that the coating has good impact resistance. From the comparison between Example 4 and Example 1, it can be seen that the use of adhesion promoter-2 may make the surface pretreatment active agent easy to absorb water, resulting in a decrease in adhesion 1 and adhesion 2, and the impact resistance of the coating decreases; from the comparison between Example 5 and Example 1, it can be seen that the use of adhesion promoter-3 may make the phosphate group content in the surface pretreatment active agent lower, resulting in a decrease in adhesion 1 and a decrease in the impact resistance of the coating; from the comparison between Example 6 and Example 1, it can be seen that the use of adhesion promoter-4 may It can reduce the content of phosphate groups and double bonds in the surface pretreatment active agent, resulting in a decrease in the levels of adhesion 1 and adhesion 2, and a decrease in the impact resistance of the coating; from the comparison between Example 7 and Example 1, it can be seen that when the conventional commercially available adhesion promoter-5 is used, the levels of adhesion 1 and adhesion 2 are lower, resulting in a decrease in the impact resistance of the coating; from the comparison between Example 8 and Example 1, it can be seen that the use of modified polyurethane acrylate-2 may make it difficult for the modified cellulose whiskers in the surface pretreatment active agent to form a random arrangement, resulting in a decrease in adhesion 2 and a decrease in the impact resistance of the coating; from the comparison between Comparative Example 1 and Example 1, it can be seen that the adhesion and impact resistance of the coating are poor when unmodified polyurethane acrylate is added.
[0100] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A surface pretreatment activator, characterized in that: The invention comprises the following raw materials in parts by weight: 30-50 parts of modified polyurethane acrylate, 4-6 parts of adhesion promoter, 1-2 parts of coupling agent and 1-2 parts of photoinitiator.
2. The surface pretreatment activator according to claim 1, characterized in that The preparation method of the modified polyurethane acrylate comprises the following steps: S1. Add cellulose whiskers and acetone into a reaction vessel, stir for 20-30 minutes, add isophorone diisocyanate, heat to 70-80°C and react for 1-2 hours, cool to room temperature, add isoamyl alcohol for precipitation, wash, filter and dry the precipitate to obtain modified cellulose whiskers; S2, adding isophorone diisocyanate, polytetramethylene glycol, the modified cellulose whisker obtained in step S1 and a catalyst into a reaction container, reacting at 70-80° C. for 1-2 hours, cooling to 50-60° C., adding a chain extender, continuing the reaction for 0.5-1 hour, adding pentaerythritol triacrylate, and reacting for 1-2 hours to obtain modified polyurethane acrylate.
3. The surface pretreatment activator according to claim 2, characterized in that: The length of the cellulose whiskers is 100-500 nm.
4. The surface pretreatment activator according to claim 2, characterized in that: The mass ratio of the modified cellulose whiskers to the chain extender is (0.6-0.7):
1.
5. The surface pretreatment activator according to claim 1, characterized in that: The preparation method of the adhesion promoter comprises the following steps: A1. Add hydroxyethyl methacrylate, gluconolactone and stannous octoate into a reaction vessel, and stir at 150-170° C. for 3-6 hours to obtain polygluconolactone containing double bonds; A2. Add the double-bond polygluconolactone obtained in step A1 and phosphoric acid into a reaction vessel, heat to 70-80° C., and react for 2-4 hours to obtain an adhesion promoter.
6. The surface pretreatment activator according to claim 5, characterized in that: The number average molecular weight of the adhesion promoter is 400-700.
7. The surface pretreatment activator according to claim 5, characterized in that: The mass ratio of hydroxyethyl methacrylate to gluconolactone is 1:(2.5-3.5).
8. The surface pretreatment activator according to claim 5, characterized in that: The mass ratio of the double-bond-containing polyglucoside lactone to phosphoric acid is 1:(0.6-0.7).
9. The surface pretreatment activator according to claim 1, characterized in that: The photoinitiator is one or more of TPO, photoinitiator 2959, photoinitiator 184, photoinitiator 1173, and photoinitiator 651.
10. A method for preparing the surface pretreatment active agent according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing modified polyurethane acrylate, adhesion promoter, coupling agent and photoinitiator, and stirring at 25-30° C. for 20-30 minutes to obtain the product.
Citation Information
Patent Citations
Nano cellulose whisker grafted water-diluted photocuring PUV (polyurethane acrylate) resin, and preparation and application thereof
CN105601878A
Adsorption promoter for photosensitive weld retarding agent
CN1077470A
Glucose-modified environment-friendly coating and preparation method thereof
CN108117782A
Accelerator and surface treatment method
CN111484800A
Weather-resistant polyurethane waterproof agent and preparation method thereof
CN118221903A