Ultraviolet curing anti-static coating and preparation method thereof

By using a combination of silicon-containing polyurethane emulsion and modified polyaniline in UV curing coatings, a high crosslink density network structure and hydrogen bond are formed, which solves the problem of insufficient hiding and adhesion of existing coatings and achieves high heat resistance The properties and adhesion meet the high requirements of solid paint.

CN118931368AInactive Publication Date: 2024-11-12SUZHOU NAPLES NANOMATERIALS CO LTD

Patent Information

Application Number
CN202411124904.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ultraviolet curing coatings have problems of insufficient hiding and adhesion in the furniture field, which is difficult to meet the high requirements of solid paints.

Method used

Using a combination of silicon-containing polyurethane emulsion and modified polyaniline, the hyperbranched polyurethane prepolymer reacts with hydroxy nanosilica, hydroxy acrylate, and diisocyanate to form a high crosslink density network structure, and high epoxy through phosphorylation Hydroxyacrylic acid is copolymerized with aniline, reducing the rigidity of the molecular chain skeleton and forming hydrogen bonds to improve the heat resistance and adhesion of the coating.

Benefits of technology

It significantly improves the adhesion and heat resistance of the paint, and meets the high requirements of solid UV curing paint in the furniture field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an ultraviolet curing antistatic coating and a preparation method thereof, and relates to the technical field of coating preparation. The ultraviolet curing anti-static coating comprises the silicon-containing polyurethane emulsion and the modified polyaniline, the silicon-containing polyurethane emulsion is prepared by reacting hyperbranched polyurethane prepolymer with hydroxyl nano-silica, hydroxyl acrylate and diisocyanate and then reacting with methylated amino resin, the adhesive force of a coating is enhanced, and the ultraviolet curing anti-static coating has the advantages that the ultraviolet curing anti-static coating is good in anti-static performance and good in anti-static performance. The heat resistance of the coating is improved, and the modified polyaniline is prepared by copolymerizing phosphorylated epoxy high-hydroxyl acrylic acid and aniline; the phosphorylated epoxy high-hydroxyl acrylic acid is prepared by polymerizing methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methylacrylate and 4-hydroxybutyl acrylate and then reacting with phosphoric acid and epoxy chloropropane, so that the heat resistance of the coating is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, in particular to an ultraviolet light-cured antistatic coating and a preparation method thereof. Background Art

[0002] UV-curing coatings have been increasingly used in the furniture field in recent years due to their advantages such as short recoating time and high production efficiency. With the official application, the requirements for UV-curing coatings are getting higher and higher, such as the transformation from transparent UV-curing coatings to solid color UV-curing coatings. By selecting different active monomers and photoinitiator synthesis formulas, the problems of hiding power and adhesion in the existing furniture coating light-curing paint technology are overcome. It can be used for roller coating, curtain coating, spray coating and other processes.

[0003] This is mainly because the photocurable coating needs to absorb ultraviolet light and then the photoinitiator is excited to produce a large number of free radical groups. These free radicals or ions react with the double bonds in the prepolymer or unsaturated monomer to form monomer genes, thereby initiating polymerization, crosslinking and grafting reactions, so that the coating is converted from liquid to solid within seconds. Therefore, the present invention studies and prepares a UV-curable antistatic coating to further solve this problem. Summary of the invention

[0004] The object of the present invention is to provide a UV-curable antistatic coating and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a UV-curable antistatic coating, comprising a silicon-containing polyurethane emulsion, modified polyaniline, a photoinitiator, a defoamer, a leveling agent and an active diluent, wherein the modified polyaniline is prepared by copolymerizing phosphorylated epoxy high-hydroxy acrylic acid with aniline.

[0006] Preferably, the silicon-containing polyurethane emulsion is prepared by reacting a hyperbranched polyurethane prepolymer with hydroxy nano-silica, hydroxy acrylate, and diisocyanate, and then reacting with a methyl etherified amino resin.

[0007] Preferably, the phosphorylated epoxy high-hydroxy acrylic acid is prepared by polymerizing methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, and then reacting with phosphoric acid and epichlorohydrin.

[0008] Preferably, the photoinitiator is one of photoinitiator TPO, photoinitiator 1173, and photoinitiator 184; the active diluent is one of tripropylene glycol diacrylate and trimethylolpropane triacrylate; the defoamer is polyether-modified polysiloxane; and the leveling agent is isophorone.

[0009] Preferably, the UV-curable antistatic coating and the preparation method thereof comprise the following specific steps: S1. In a nitrogen atmosphere, diisocyanate and hydroxy nano-silica were mixed in a mass ratio of 8-10:1, heated to 58-62°C, reacted for 2-4 hours, cooled to room temperature, and a mixture of 4-8% hydroxyethyl acrylate and 0.02-0.04% p-methoxyphenol, a polymerization inhibitor, was added dropwise at a rate of 1-3 ml / min. The mass ratio of hydroxyethyl acrylate to p-methoxyphenol was 10:1. 0~200:1, heat to 40~42℃, keep warm for 2~4h, add hyperbranched polyurethane prepolymer with 4~6 times the mass of hydroxy nano-silicon dioxide, heat to 64~66℃, continue to react for 2~4h, then add methyl etherified amino resin with 0.3~0.4 times the mass of hydroxy nano-silicon dioxide, and add concentrated sulfuric acid with 0.2~0.4 times the mass of methyl etherified amino resin dropwise at a rate of 1~3ml / min, continue to react for 2~4h, and obtain silicon-containing polyurethane emulsion; S2. High hydroxy acrylic acid, phosphoric acid, urea and deionized water are mixed in a mass ratio of 1:2~4:0.3~0.5:50, heated to 48~50°C, kept warm for 7~9h, heated to 94~96°C, kept warm for 4~6h, washed with anhydrous ethanol, dissolved with deionized water, adjusted the pH to 10.8~11.2 with potassium hydroxide, added epichlorohydrin 2~4 times the mass of high hydroxy acrylic acid at a rate of 1~3ml / min, heated to 75~85°C, reacted for 2~4h, and obtained phosphorylated epoxy high hydroxy acrylic acid; S3. Add aniline in an amount of 0.8 to 1.2 times the mass of the phosphated epoxy high hydroxy acrylic acid to the phosphated epoxy high hydroxy acrylic acid, react for 2 to 3 hours, transfer to an ice bath, adjust the pH to 1 to 2 with hydrochloric acid, then add initiator ammonium persulfate in an amount of 0.02 to 0.08 times the mass of the aniline, react for 24 to 28 hours, and finally dialyze with a dialysis bag to obtain modified polyaniline; S4. Mix the silicon-containing polyurethane emulsion, modified polyaniline and active diluent, add the photoinitiator after stirring evenly, add the defoamer and leveling agent after they are dissolved, and stir evenly to obtain a UV-curable antistatic coating.

[0010] Preferably, in the above step S1., the preparation method of hydroxy nano-silica is: sodium metasilicate and deionized water are mixed in a mass ratio of 1-4:50, and after stirring evenly, 4-8% hydrochloric acid with a mass fraction of 2-6 times the mass of sodium metasilicate is added dropwise at a rate of 1-3 ml / min, reacting for 4-6 hours and then filtering, washing with ethanol and deionized water for 3-5 times in sequence, spray drying, and the outlet temperature is 140-160°C, grinding, and obtaining hydroxy nano-silica.

[0011] Preferably, in the above step S1., the preparation method of the hyperbranched polyurethane prepolymer is: under a nitrogen atmosphere, isophorone diisocyanate and a catalyst T-12 with a mass fraction of 6-8% are mixed in a mass ratio of 10:0.1-0.4, the temperature is raised to 44-46°C, pentaerythritol with a mass of 4-6 times that of isophorone diisocyanate is added dropwise at a rate of 1-3 ml / min, the temperature is raised to 54-56°C, the reaction is kept warm for 3-6 hours, and the hyperbranched polyurethane prepolymer is obtained by drying.

[0012] Preferably, in the above step S2., the preparation method of high hydroxy acrylic acid is: emulsion, emulsifier OP-10, initiator ammonium persulfate, deionized water and sodium bicarbonate are mixed in a mass ratio of 10:0.2:0.05~0.1:4:1, and after keeping warm for 30~40 minutes, emulsion 2~4 times the mass of sodium bicarbonate is added dropwise at a rate of 1~3 ml / min, and the reaction is kept warm for 2~3 hours, and the temperature is reduced to 45~48°C, and the pH is adjusted to 7~8 with ammonia water to obtain high hydroxy acrylic acid.

[0013] Preferably, the emulsion is prepared by mixing emulsifier OP-10, initiator ammonium persulfate and deionized water in a mass ratio of 2:1:50-80, adding methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, and the mass ratio of emulsifier OP-10, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate is 0.2-0.4:6:8:8:12:9, and stirring evenly.

[0014] Preferably, in the above step S4., the mass ratio of the silicon-containing polyurethane emulsion, the modified polyaniline, the photoinitiator, the defoaming agent, the leveling agent and the reactive diluent is 8-10:1-2:0.04-0.08:0.01:0.01:0.01-0.03.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The ultraviolet light curing antistatic coating prepared by the invention comprises a silicon-containing polyurethane emulsion and modified polyaniline; The silicon-containing polyurethane emulsion is prepared by reacting a hyperbranched polyurethane prepolymer with hydroxy nano-silicon dioxide, hydroxy acrylate, and diisocyanate, and then reacting with a methyl etherified amino resin; sodium metasilicate is hydrolyzed to generate silicic acid, which undergoes dehydration and polycondensation, and bonds with silicon oxygen bonds, so that the surface of the nano-silicon dioxide has a large number of hydroxyl groups, and then reacts with the hyperbranched polyurethane prepolymer, hydroxy acrylate, and diisocyanate to form a polyurethane acrylate emulsion containing nano-silicon dioxide and having a hyperbranched structure, and the nano-silicon dioxide is evenly linked in the hyperbranched structure, so that the hardness of the polyurethane acrylate is reduced and the adhesion of the coating is enhanced, and then reacts with the methyl etherified amino resin, and a cross-linking agent is introduced into the hyperbranched structure, so that a high cross-linking density network structure can be formed in the silicon-containing polyurethane emulsion, and the heat resistance of the coating is improved; Modified polyaniline is prepared by copolymerization of phosphorylated epoxy high hydroxy acrylic acid and aniline; phosphorylated epoxy high hydroxy acrylic acid is prepared by polymerization of methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, and then grafted copolymerized with phosphoric acid and epichlorohydrin and aniline to obtain modified polyaniline, which reduces the rigidity of the molecular chain skeleton, so that the modified polyaniline added to the coating can not only prevent static electricity, but also form hydrogen bonds with the silicon-containing polyurethane emulsion, and is coated on a high cross-linking density network structure, further improving the heat resistance of the coating. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the UV-curable antistatic coatings prepared in the examples and comparative examples as follows: Peel strength: The adhesion test of the UV-curable antistatic coatings prepared in the examples and comparative examples was performed with reference to GB5210.

[0018] Heat resistance: The UV-curable antistatic coatings prepared in the embodiment and the comparative example were coated on the same material surface with the same amount and thickness. After UV curing for the same time, a heat resistance test was carried out at 150°C for 120 hours in accordance with GB / T1735.

[0019] Example 1

[0020] S1. In a nitrogen atmosphere, isophorone diisocyanate and 6% catalyst T-12 were mixed in a mass ratio of 10:0.1, the temperature was raised to 44°C, pentaerythritol 4 times the mass of isophorone diisocyanate was added dropwise at a rate of 1 ml / min, the temperature was raised to 54°C, the reaction was kept warm for 3 hours, and a hyperbranched polyurethane prepolymer was obtained by drying; sodium metasilicate and deionized water were mixed in a mass ratio of 1:50, and after stirring, 4% hydrochloric acid 2 times the mass of sodium metasilicate was added dropwise at a rate of 1 ml / min, the reaction was carried out for 4 hours, and then filtered, washed with ethanol and deionized water for 3 times, spray dried, and the outlet temperature was 140°C, and ground to obtain hydroxy nano-silica; diisocyanate and hydroxy nano-silica were mixed in a nitrogen atmosphere. The silica was mixed in a mass ratio of 8:1, heated to 58°C, reacted for 2 hours, cooled to room temperature, and a mixed solution of 4% hydroxyethyl acrylate and 0.02% p-methoxyphenol, an inhibitor, was added dropwise at a rate of 1 ml / min, the mass ratio of hydroxyethyl acrylate to p-methoxyphenol being 100:1, heated to 40°C, kept warm for 2 hours, and a hyperbranched polyurethane prepolymer of 4 times the mass of hydroxy nano-silica was added, heated to 64°C, continued to react for 2 hours, and then 0.3 times the mass of methyl etherified amino resin was added, and 0.2 times the mass of methyl etherified amino resin was added dropwise at a rate of 1 ml / min, and continued to react for 2 hours to obtain a silicon-containing polyurethane emulsion; S2. After the emulsifier OP-10, the initiator ammonium persulfate and deionized water are mixed in a mass ratio of 2:1:50, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, 4-hydroxybutyl acrylate are added, and the mass ratio of emulsifier OP-10, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, and 4-hydroxybutyl acrylate is 0.2:6:8:8:12:9, and stirred to obtain an emulsion; the emulsion, emulsifier OP-10, initiator ammonium persulfate, deionized water and sodium bicarbonate are mixed in a mass ratio of 10:0.2:0.05:4:1, and the mixture is kept warm for 30 min later, add an emulsion twice the mass of sodium bicarbonate at a rate of 1 ml / min, keep warm for 2 h, cool to 45°C, adjust the pH to 7 with ammonia water, and obtain high-hydroxy acrylic acid; mix high-hydroxy acrylic acid, phosphoric acid, urea and deionized water in a mass ratio of 1:2:0.3:50, heat to 48°C, keep warm for 7 h, heat to 94°C, continue to keep warm for 4 h, wash with anhydrous ethanol, dissolve with deionized water, adjust the pH to 10.8 with potassium hydroxide, add epichlorohydrin twice the mass of high-hydroxy acrylic acid at a rate of 1 ml / min, heat to 75°C, react for 2 h, and obtain phosphorylated epoxy high-hydroxy acrylic acid; S3. Add aniline in an amount of 0.8 times the mass of the phosphorylated epoxy high hydroxy acrylic acid to the phosphorylated epoxy high hydroxy acrylic acid, react for 2 hours, transfer to an ice bath, adjust the pH to 1 with hydrochloric acid, then add ammonium persulfate as an initiator in an amount of 0.02 times the mass of the aniline, react for 24 hours, and finally dialyze with a dialysis bag to obtain modified polyaniline; S4. Mix the silicon-containing polyurethane emulsion, modified polyaniline and reactive diluent, add the photoinitiator after stirring evenly, add the defoamer and leveling agent after dissolution, and stir evenly. The mass ratio of the silicon-containing polyurethane emulsion, modified polyaniline, photoinitiator, defoamer, leveling agent and reactive diluent is 8:1:0.04:0.01:0.01:0.01 to obtain a UV-curable antistatic coating.

[0021] Example 2

[0022] S1. In a nitrogen atmosphere, isophorone diisocyanate and 7% catalyst T-12 were mixed in a mass ratio of 10:0.25, the temperature was raised to 45°C, pentaerythritol 5 times the mass of isophorone diisocyanate was added dropwise at a rate of 2 ml / min, the temperature was raised to 55°C, the reaction was kept warm for 4.5 hours, and a hyperbranched polyurethane prepolymer was obtained by drying; sodium metasilicate and deionized water were mixed in a mass ratio of 3:50, stirred evenly, and 6% hydrochloric acid 4 times the mass of sodium metasilicate was added dropwise at a rate of 2 ml / min, the reaction was carried out for 5 hours, and then filtered, washed with ethanol and deionized water 4 times in turn, spray dried, and the outlet temperature was 150°C, and ground to obtain hydroxy nano-silica; diisocyanate and hydroxy nano-silica were mixed in a nitrogen atmosphere. The silica was mixed in a mass ratio of 9:1, heated to 60°C, reacted for 3 hours, cooled to room temperature, and a mixed solution of 6% hydroxyethyl acrylate with a mass fraction of 3 times the mass of diisocyanate and 0.03% of the mass fraction of para-methoxyphenol as a polymerization inhibitor was added dropwise at a rate of 2 ml / min, the mass ratio of hydroxyethyl acrylate to para-methoxyphenol as a polymerization inhibitor was 150:1, heated to 41°C, kept warm for 3 hours, and a hyperbranched polyurethane prepolymer with a mass fraction of 5 times that of hydroxy nano-silica was added, heated to 65°C, continued to react for 3 hours, and then methyl etherified amino resin with a mass fraction of 0.35 times that of hydroxy nano-silica was added, and concentrated sulfuric acid with a mass fraction of 0.3 times that of the methyl etherified amino resin was added dropwise at a rate of 2 ml / min, and continued to react for 3 hours to obtain a silicon-containing polyurethane emulsion; S2. After the emulsifier OP-10, the initiator ammonium persulfate and deionized water are mixed in a mass ratio of 2:1:65, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, 4-hydroxybutyl acrylate are added, and the mass ratio of emulsifier OP-10, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, and 4-hydroxybutyl acrylate is 0.3:6:8:8:12:9, and the emulsion is stirred to obtain an emulsion; the emulsion, emulsifier OP-10, initiator ammonium persulfate, deionized water and sodium bicarbonate are mixed in a mass ratio of 10:0.2:0.08:4:1, and the mixture is kept warm for 35 minutes. Then, add an emulsion 34 times the mass of sodium bicarbonate at a rate of 2 ml / min, keep warm for 2.5 hours, cool to 46°C, adjust the pH to 7.5 with ammonia water to obtain high-hydroxy acrylic acid; mix high-hydroxy acrylic acid, phosphoric acid, urea and deionized water in a mass ratio of 1:3:0.4:50, heat to 49°C, keep warm for 8 hours, heat to 95°C, continue to keep warm for 5 hours, wash with anhydrous ethanol, dissolve with deionized water, adjust the pH to 11.0 with potassium hydroxide, add epichlorohydrin 3 times the mass of high-hydroxy acrylic acid at a rate of 2 ml / min, heat to 80°C, react for 3 hours, and obtain phosphorylated epoxy high-hydroxy acrylic acid; S3. Add aniline (1 times the mass of phospho-epoxy high-hydroxy acrylic acid) to the phosphorylated epoxy high-hydroxy acrylic acid, react for 2.5 hours, transfer to an ice bath, adjust the pH to 1.5 with hydrochloric acid, then add ammonium persulfate (0.05 times the mass of aniline) as an initiator, react for 26 hours, and finally dialyze with a dialysis bag to obtain modified polyaniline; S4. Mix the silicon-containing polyurethane emulsion, modified polyaniline and active diluent, add the photoinitiator after stirring evenly, add the defoamer and leveling agent after dissolution, and stir evenly. The mass ratio of the silicon-containing polyurethane emulsion, modified polyaniline, photoinitiator, defoamer, leveling agent and active diluent is 9:1.5:0.06:0.01:0.01:0.02 to obtain a UV-curable antistatic coating.

[0023] Example 3

[0024] S1. In a nitrogen atmosphere, isophorone diisocyanate and 8% catalyst T-12 are mixed in a mass ratio of 10:0.4, the temperature is raised to 46°C, pentaerythritol (6 times the mass of isophorone diisocyanate) is added dropwise at a rate of 3 ml / min, the temperature is raised to 56°C, the reaction is kept warm for 6 hours, and a hyperbranched polyurethane prepolymer is obtained by drying; sodium metasilicate and deionized water are mixed in a mass ratio of 4:50, and after stirring, 8% hydrochloric acid (6 times the mass of sodium metasilicate) is added dropwise at a rate of 3 ml / min, the reaction is carried out for 6 hours, and then filtered, washed with ethanol and deionized water for 5 times in sequence, spray dried, and the outlet temperature is 160°C, and ground to obtain hydroxy nano-silica; diisocyanate and hydroxy nano-silica are mixed in a nitrogen atmosphere, and the mixture is stirred at a temperature of 150°C. Silicon is mixed in a mass ratio of 10:1, heated to 62°C, reacted for 4 hours, cooled to room temperature, and a mixed solution of 8% hydroxyethyl acrylate and 0.04% p-methoxyphenol, a polymerization inhibitor, is added dropwise at a rate of 3 ml / min, the mass ratio of hydroxyethyl acrylate to p-methoxyphenol is 200:1, heated to 42°C, kept warm for 4 hours, and a hyperbranched polyurethane prepolymer is added in an amount of 6 times the mass of hydroxy nano-silica, heated to 66°C, and reacted for 4 hours, and then a methyl etherified amino resin in an amount of 0.4 times the mass of hydroxy nano-silica is added, and concentrated sulfuric acid in an amount of 0.2-0.4 times the mass of the methyl etherified amino resin is added dropwise at a rate of 3 ml / min, and the reaction is continued for 4 hours to obtain a silicon-containing polyurethane emulsion; S2. After the emulsifier OP-10, the initiator ammonium persulfate and deionized water are mixed in a mass ratio of 2:1:80, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, 4-hydroxybutyl acrylate are added, the mass ratio of emulsifier OP-10, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate, 4-hydroxybutyl acrylate is 0.4:6:8:8:12:9, and the emulsion is stirred to obtain an emulsion; the emulsion, emulsifier OP-10, initiator ammonium persulfate, deionized water and sodium bicarbonate are mixed in a mass ratio of 10:0.2:0.1:4:1, and the mixture is kept warm for 40min. n, dripping an emulsion 4 times the mass of sodium bicarbonate at a rate of 3 ml / min, keeping the temperature for reaction for 3 hours, cooling to 48°C, adjusting the pH to 8 with ammonia water, and obtaining high-hydroxy acrylic acid; mixing high-hydroxy acrylic acid, phosphoric acid, urea and deionized water in a mass ratio of 1:4:0.5:50, heating to 50°C, keeping the temperature for 9 hours, heating to 96°C, and continuing to keep the temperature for 6 hours, washing with anhydrous ethanol, and then dissolving with deionized water, adjusting the pH to 11.2 with potassium hydroxide, dripping epichlorohydrin 4 times the mass of high-hydroxy acrylic acid at a rate of 1-3 ml / min, heating to 85°C, and reacting for 4 hours, and obtaining phosphorylated epoxy high-hydroxy acrylic acid; S3. Add aniline in an amount of 1.2 times the mass of phospho-epoxy high-hydroxy acrylic acid to the phosphorylated epoxy high-hydroxy acrylic acid, react for 3 hours, transfer to an ice bath, adjust the pH to 2 with hydrochloric acid, then add ammonium persulfate as an initiator in an amount of 0.08 times the mass of aniline, react for 28 hours, and finally dialyze with a dialysis bag to obtain modified polyaniline; S4. Mix the silicon-containing polyurethane emulsion, modified polyaniline and reactive diluent, add the photoinitiator after stirring evenly, add the defoamer and leveling agent after dissolution, and stir evenly. The mass ratio of the silicon-containing polyurethane emulsion, modified polyaniline, photoinitiator, defoamer, leveling agent and reactive diluent is 10:2:0.08:0.01:0.01:0.03 to obtain a UV-curable antistatic coating.

[0025] Comparative Example 1 The composition of comparative example 1 is the same as that of example 2. The difference between the preparation method of the UV-curable antistatic coating and that of example 2 is that the silicon-containing polyurethane emulsion is prepared by reacting a hyperbranched polyurethane prepolymer with hydroxy nano-silica, hydroxy acrylate, and diisocyanate.

[0026] Comparative Example 2 The composition of Comparative Example 2 is the same as that of Example 2. The difference between the preparation method of the UV-curable antistatic coating and that of Example 2 is that the modified polyaniline is prepared by copolymerization of high-hydroxy acrylic acid and aniline.

[0027] Comparative Example 3 The composition of Comparative Example 3 is the same as that of Example 2. The difference between the preparation method of the UV-curable antistatic coating and that of Example 2 is that the UV-curable antistatic coating only includes polyurethane emulsion, modified polyaniline, photoinitiator, defoamer, leveling agent and reactive diluent.

[0028] Comparative Example 4 The composition of Comparative Example 4 is the same as that of Example 2. The difference between the preparation method of the UV-curable antistatic coating and that of Example 2 is that the UV-curable antistatic coating comprises a silicon-containing polyurethane emulsion, polyaniline, a photoinitiator, a defoamer, a leveling agent and a reactive diluent.

[0029] Comparative Example 5 The composition of Comparative Example 5 is the same as that of Example 2. The difference between the preparation method of the UV-curable antistatic coating and that of Example 2 is that the UV-curable antistatic coating only includes silicon-containing polyurethane emulsion, photoinitiator, defoamer, leveling agent and reactive diluent.

[0030] Effect example Table 1 below shows the performance analysis results of the UV-curable antistatic coatings prepared using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5:

[0031] By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the UV-curable antistatic coatings prepared using Examples 1, 2, and 3 have excellent peel strength and heat resistance.

[0032] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1 and Comparative Example 3, it can be found that after the hyperbranched polyurethane prepolymer reacts with hydroxy nano-silicon dioxide, hydroxy acrylate, and diisocyanate, the silicon-containing polyurethane emulsion obtained by reacting with methyl etherified amino resin, sodium metasilicate is hydrolyzed to generate silicic acid, which undergoes dehydration and polycondensation, and bonds with silicon oxygen bonds, so that the surface of the nano-silicon dioxide has a large number of hydroxyl groups, and reacts with the hyperbranched polyurethane prepolymer, hydroxy acrylate, and diisocyanate to form a polyurethane acrylate emulsion containing nano-silicon dioxide and having a hyperbranched structure, and the nano-silicon dioxide is evenly linked in the hyperbranched structure, the hardness of the polyurethane acrylate is reduced, and the adhesion of the coating is enhanced, and then the hyperbranched amino resin is reacted to introduce a cross-linking agent into the hyperbranched structure, so that a high cross-linking density network structure can be formed in the silicon-containing polyurethane emulsion, thereby improving the heat resistance of the coating.

[0033] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 2, Comparative Example 4, Comparative Example 5, it can be found that the modified polyaniline prepared by polymerization of methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, phosphoric acid and epichlorohydrin to prepare phosphorylated epoxy high-hydroxy acrylic acid, and aniline, reduces the rigidity of the molecular chain skeleton, so that the modified polyaniline added to the coating can not only prevent static electricity, but also form hydrogen bonds with the silicon-containing polyurethane emulsion, and is coated on the high cross-linking density network structure, further improving the heat resistance of the coating.

[0034] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A UV-curable antistatic coating, characterized in that: The invention comprises silicon-containing polyurethane emulsion, modified polyaniline, photoinitiator, defoamer, leveling agent and active diluent; the modified polyaniline is prepared by copolymerization of phosphorylated epoxy high-hydroxy acrylic acid and aniline.

2. The UV-curable antistatic coating according to claim 1, characterized in that: The silicon-containing polyurethane emulsion is prepared by reacting a hyperbranched polyurethane prepolymer with hydroxy nano silicon dioxide, hydroxy acrylic acid ester and diisocyanate, and then reacting with methyl etherified amino resin.

3. The UV-curable antistatic coating according to claim 1, characterized in that: The phosphorylated epoxy high-hydroxy acrylic acid is prepared by polymerizing methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, and then reacting with phosphoric acid and epichlorohydrin.

4. The UV-curable antistatic coating according to claim 1, characterized in that: The photoinitiator is one of photoinitiator TPO, photoinitiator 1173, and photoinitiator 184; the active diluent is one of tripropylene glycol diacrylate and trimethylolpropane triacrylate; the defoamer is polyether-modified polysiloxane; and the leveling agent is isophorone.

5. A method for preparing the UV-curable antistatic coating according to claim 1, characterized in that: The specific steps include: S1. In a nitrogen atmosphere, diisocyanate and hydroxy nano-silica were mixed in a mass ratio of 8-10:1, heated to 58-62°C, reacted for 2-4 hours, cooled to room temperature, and a mixture of 4-8% hydroxyethyl acrylate and 0.02-0.04% p-methoxyphenol, a polymerization inhibitor, was added dropwise at a rate of 1-3 ml / min. The mass ratio of hydroxyethyl acrylate to p-methoxyphenol was 10:

1. 0~200:1, heat to 40~42℃, keep warm for 2~4h, add hyperbranched polyurethane prepolymer with 4~6 times the mass of hydroxy nano-silicon dioxide, heat to 64~66℃, continue to react for 2~4h, then add methyl etherified amino resin with 0.3~0.4 times the mass of hydroxy nano-silicon dioxide, and add concentrated sulfuric acid with 0.2~0.4 times the mass of methyl etherified amino resin dropwise at a rate of 1~3ml / min, continue to react for 2~4h, and obtain silicon-containing polyurethane emulsion; S2. High hydroxy acrylic acid, phosphoric acid, urea and deionized water are mixed in a mass ratio of 1:2~4:0.3~0.5:50, heated to 48~50°C, kept warm for 7~9h, heated to 94~96°C, kept warm for 4~6h, washed with anhydrous ethanol, dissolved with deionized water, adjusted the pH to 10.8~11.2 with potassium hydroxide, added epichlorohydrin 2~4 times the mass of high hydroxy acrylic acid at a rate of 1~3ml / min, heated to 75~85°C, reacted for 2~4h, and obtained phosphorylated epoxy high hydroxy acrylic acid; S3. Add aniline in an amount of 0.8 to 1.2 times the mass of the phosphated epoxy high hydroxy acrylic acid to the phosphated epoxy high hydroxy acrylic acid, react for 2 to 3 hours, transfer to an ice bath, adjust the pH to 1 to 2 with hydrochloric acid, then add initiator ammonium persulfate in an amount of 0.02 to 0.08 times the mass of the aniline, react for 24 to 28 hours, and finally dialyze with a dialysis bag to obtain modified polyaniline; S4. Mix the silicon-containing polyurethane emulsion, modified polyaniline and active diluent, add the photoinitiator after stirring evenly, add the defoamer and leveling agent after they are dissolved, and stir evenly to obtain a UV-curable antistatic coating.

6. The method for preparing a UV-curable antistatic coating according to claim 5, characterized in that: In the above step S1., the preparation method of hydroxy nano-silica is: sodium metasilicate and deionized water are mixed in a mass ratio of 1-4:50, and after stirring evenly, 4-8% hydrochloric acid with a mass fraction of 2-6 times the mass of sodium metasilicate is added dropwise at a rate of 1-3 ml / min, reacting for 4-6 hours and then filtering, washing with ethanol and deionized water for 3-5 times in sequence, spray drying, the outlet temperature is 140-160°C, grinding, and obtaining hydroxy nano-silica.

7. The method for preparing a UV-curable antistatic coating according to claim 5, characterized in that: In the above step S1., the preparation method of the hyperbranched polyurethane prepolymer is as follows: under a nitrogen atmosphere, isophorone diisocyanate and a catalyst T-12 with a mass fraction of 6-8% are mixed in a mass ratio of 10:0.1-0.4, the temperature is raised to 44-46°C, pentaerythritol with a mass of 4-6 times that of isophorone diisocyanate is added dropwise at a rate of 1-3 ml / min, the temperature is raised to 54-56°C, the reaction is kept warm for 3-6 hours, and the hyperbranched polyurethane prepolymer is obtained by drying.

8. The method for preparing a UV-curable antistatic coating according to claim 5, characterized in that: In the above step S2., the preparation method of high hydroxy acrylic acid is: emulsion, emulsifier OP-10, initiator ammonium persulfate, deionized water and sodium bicarbonate are mixed in a mass ratio of 10:0.2:0.05~0.1:4:1, and after keeping warm for 30~40 minutes, emulsion 2~4 times the mass of sodium bicarbonate is added dropwise at a rate of 1~3 ml / min, and the reaction is kept warm for 2~3 hours, and the temperature is reduced to 45~48°C, and the pH is adjusted to 7~8 with ammonia water to obtain high hydroxy acrylic acid.

9. The method for preparing a UV-curable antistatic coating according to claim 8, characterized in that: The emulsion is prepared by mixing an emulsifier OP-10, an initiator ammonium persulfate and deionized water in a mass ratio of 2:1:50-80, adding methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate, wherein the mass ratio of the emulsifier OP-10, methyl methacrylate, n-butyl acrylate, acrylic acid, hydroxyethyl methacrylate and 4-hydroxybutyl acrylate is 0.2-0.4:6:8:8:12:9, and stirring evenly.

10. The method for preparing a UV-curable antistatic coating according to claim 5, characterized in that: In the above step S4., the mass ratio of the silicon-containing polyurethane emulsion, the modified polyaniline, the photoinitiator, the defoaming agent, the leveling agent and the reactive diluent is 8~10:1~2:0.04~0.08:0.01:0.01:0.01~0.03.

Citation Information

Patent Citations

  • Aqueous system conductive polyaniline ultraviolet curing antistatic coating and preparation method thereof

    CN101955726A

  • Intrinsic anti-static hardened film and preparation method thereof

    CN103642384A

  • Method for preparing UV (Ultraviolet) cured anti-electromagnetic shielding coating based on graphene oxide

    CN103788806A

  • High strength anti-pollution UV curable paint and preparation method thereof

    CN103834291A

  • Conductive and antistatic liquid and preparation method thereof

    CN113528009A

Cited By

  • High-adhesion electrical insulation polyolefin hot melt adhesive and preparation method thereof

    CN120574539A