Temperature-resistant UV pressure-sensitive adhesive for bonding notebook computer outer frame and preparation method of temperature-resistant UV pressure-sensitive adhesive

By preparing a temperature-resistant UV pressure-sensitive adhesive for the outer frame of the notebook, the problem of insufficient weather resistance at high temperatures in the prior art is solved, and higher initial viscosity and shear force are achieved. It meets the high-temperature application needs of notebook frame bonding and replaces traditional pressure-sensitive tape.

CN118931395APending Publication Date: 2024-11-12苏州环明新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411358051.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the face of special application scenarios, especially the demand for temperature resistance, existing UV pressure-sensitive adhesives are difficult to meet the comprehensive performance requirements of high initial viscosity, rebound reworkability and high temperatures, especially in the outer frame of the notebook. Bonding field.

Method used

A temperature-resistant UV pressure-sensitive adhesive for bonding of notebook frames is used, and the formulation includes modified acrylate oligomer resin, acrylate monomer, initiator and vapor phase silica, through specific stirring and detachment. The bubble process is prepared to form an adhesive with high initial viscosity, shear force and high temperature weather resistance, replacing the traditional pressure-sensitive tape.

Benefits of technology

It achieves higher adhesion and shear force than traditional tapes, and exhibits better weather resistance at high temperatures, meets the bonding needs of the notebook industry, and achieves the improvement of automated operation processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931395A_ABST
    Figure CN118931395A_ABST
Patent Text Reader

Abstract

The invention discloses a temperature-resistant UV pressure-sensitive adhesive for bonding an outer frame of a notebook computer and a preparation method thereof, and the preparation method comprises the following steps: adding 2-5 acrylate monomers into a stirring device, starting a stirring function, and uniformly mixing at a low speed; adding an initiator, and fully stirring until the initiator is completely dissolved; adding fumed silica, dispersing and stirring at a high speed, and completely dispersing the fumed silica into the system; adding acrylate oligomer resin, stirring and dispersing at a high speed, and uniformly mixing; continuously defoaming for several times through vacuum defoaming, and then discharging through a 200-mesh filter screen, so as to obtain the temperature-resistant UV pressure-sensitive adhesive for bonding the notebook computer outer frame. The UV pressure-sensitive adhesive disclosed by the invention can have a certain initial adhesion force, replaces the application of a traditional pressure-sensitive adhesive tape, is relatively good in cohesion force, and does not affect the reworkability of a process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pressure-sensitive adhesive preparation, and in particular to a temperature-resistant UV pressure-sensitive adhesive for bonding notebook outer frames and a preparation method thereof. Background Art

[0002] In recent years, the demand for UV adhesives in industrial applications has increased year by year. They are favored by the majority of users due to their advantages such as being solvent-free and environmentally friendly during preparation and use. UV adhesives have a short curing time and occupy a small space, which can meet today's refined and continuous automated production requirements. Among the types of UV adhesives, there is a type of UV pressure-sensitive adhesive, which has fewer application areas; currently, the main application market is solvent-based acrylic pressure-sensitive tapes. Conventional UV pressure-sensitive adhesives mainly have basic requirements for initial adhesion and peel strength, but less research is done on the rebound, reworkability, and temperature resistance of the application. Faced with special application scenario requirements, especially in technical fields with high requirements for temperature resistance, it is difficult for conventional UV pressure-sensitive adhesives to meet their comprehensive performance.

[0003] Therefore, in response to the above problems, the present invention provides a temperature-resistant UV pressure-sensitive adhesive for notebook frame bonding and a preparation method thereof, a UV pressure-sensitive adhesive with relatively high initial adhesion, high strength and resilience, whose weather resistance at high and low temperatures can replace the performance of pressure-sensitive tape, meet its bonding needs in the notebook industry, replace the use of tape, and thus solve the bottleneck problem of the automated operation process in this process. Summary of the invention

[0004] The purpose of the present invention is to provide a temperature-resistant UV pressure-sensitive adhesive for bonding notebook frames and a preparation method thereof, so as to fill the gap in the current technology.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] A heat-resistant UV pressure-sensitive adhesive for bonding notebook frames, wherein the total weight of the heat-resistant UV pressure-sensitive adhesive is 115.0 to 120.0 g, and the adhesive comprises the following components in parts by weight:

[0007] Modified acrylate oligomer resin: 40-90 parts;

[0008] Acrylate monomer: 20-60 parts;

[0009] Initiator: 1-5 parts;

[0010] Silicon dioxide: 1-5 parts;

[0011] Wherein, the silicon dioxide is fumed silicon dioxide; the modified acrylate oligomer resin is selected from one or both of a 2-functional polyacrylate oligomer resin or a 2-functional aliphatic polyurethane acrylate oligomer resin.

[0012] Preferably, the 2-functional polyacrylate oligomer resin is selected from one or more of modified acrylate oligomer resin 61363 and modified acrylate oligomer resin 61217.

[0013] Preferably, the 2-functionality aliphatic polyurethane acrylate oligomer resin is selected from one or more of GU3020Z, GU3300Z, GU3300P, and GU8366P.

[0014] Preferably, the acrylate monomer is selected from one or more of tetrahydrofuran acrylate monomer (THFA), isobornyl acrylate monomer (IBOA), isotridecyl acrylate monomer (IDTA), 4-tert-butylcyclohexyl acrylate monomer (TBCHA), 2-ethylhexyl acrylate monomer (EHA), and isooctyl acrylate (2-EHA).

[0015] Preferably, the initiator is selected from one or more of initiator methyl benzoylformate (initiator MBF), initiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (initiator TPO), initiator 184, initiator 754, and initiator 819.

[0016] A method for preparing a heat-resistant UV pressure-sensitive adhesive for bonding notebook frames, comprising the following steps:

[0017] S1. First, take 2 to 5 kinds of acrylic ester monomers and add them into a stirring device, turn on the stirring function and mix them at a low speed;

[0018] S2. After step S1 is evenly mixed, add the initiator thereto and stir thoroughly until it is completely dissolved;

[0019] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0020] S4: adding 2-functional polyacrylate oligomer resin and 2-functional aliphatic polyurethane acrylate oligomer resin, and mixing them evenly through high-speed stirring and dispersion; performing continuous degassing by vacuum degassing, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0021] Preferably, the vacuum degassing pressure is set to -0.08 MPa, and the continuous degassing is performed 2 to 3 times, each time for 10 to 12 minutes.

[0022] Preferably, the stirring device is selected from a vacuum homogenizer or a double planetary mixer.

[0023] In the above technical solution, the modified acrylate oligomer resins: 61363 and 61217 are products of Changxing Chemical; the aliphatic polyurethane acrylate oligomer resins: GU3020Z, GU3300Z, GU3300P, and GU8366P are products of Guojing Chemical.

[0024] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0025] 1. The heat-resistant UV pressure-sensitive adhesive for notebook frame bonding of the present invention is an acrylic acid + UV system pressure-sensitive adhesive. After UV curing, it has a certain initial adhesion and replaces the application of traditional pressure-sensitive tapes;

[0026] 2. The heat-resistant UV pressure-sensitive adhesive used for bonding notebook frames of the present invention has higher bonding strength and shearing force than the adhesive tape;

[0027] 3. The heat-resistant UV pressure-sensitive adhesive used for bonding notebook frames of the present invention has passed the test and has obvious advantages over the same type of tape / UV pressure-sensitive adhesive;

[0028] 4. The heat-resistant UV pressure-sensitive adhesive used for bonding notebook frames of the present invention has good cohesive force and has no influence on the reworkability of the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, some of the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be made based on these drawings without paying any creative work.

[0030] Figure 1 is a schematic diagram of a peeling force testing method according to Embodiment 1 of the present invention;

[0031] Figure 2 is a schematic diagram of a shear force testing method according to Example 1 of the present invention;

[0032] Among them, 1. PET original film; 2. UV pressure-sensitive adhesive; 3. SUS stainless steel plate. DETAILED DESCRIPTION

[0033] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, a specific implementation scheme is now described in detail.

[0034] The present invention is further described below in conjunction with the examples, but the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not indicated are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0035] Example 1

[0036] See attached Figure 1-2 This embodiment provides a method for preparing a temperature-resistant UV pressure-sensitive adhesive for bonding a notebook frame, comprising the following steps:

[0037] The UV pressure-sensitive adhesive comprises, by weight: 15 parts of IBOA, 15 parts of HEA, 20 parts of 2-EHA; 1.5 parts of initiator 754, 2.8 parts of initiator 184, 0.7 parts of initiator TPO, 55 parts of modified acrylate oligomer resin 61363, and 5 parts of fumed silica;

[0038] S1. First, add the acrylic acid ester monomers IBOA, HEA, and 2-EHA into a vacuum homogenizer according to the above weight, and start the stirring function at a low speed to mix them evenly;

[0039] S2. After step S1 is evenly mixed, initiator 754, initiator 184, and initiator TPO are added thereto in sequence, and stirred thoroughly until they are completely dissolved;

[0040] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0041] S4: adding modified acrylic oligomer resin 61363, and mixing evenly through high-speed stirring and dispersion; performing vacuum degassing with the air pressure set to -0.08 MPa, performing degassing three times, each for 10 minutes, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0042] Example 2

[0043] This embodiment provides a method for preparing a temperature-resistant UV pressure-sensitive adhesive for bonding a notebook frame, comprising the following steps:

[0044] The UV pressure-sensitive adhesive comprises, by weight: 7 parts of IBOA, 8 parts of DMAA, 7 parts of HEA, 8 parts of 2-EHA; 0.2 parts of initiator 819, 3 parts of initiator MBF, 0.8 parts of initiator TPO, 50 parts of GU3300Z, 30 parts of GU3300P, and 3 parts of fumed silica;

[0045] S1. First, add the acrylic acid ester monomers IBOA, DMAA, HEA, and 2-EHA according to the above weight into a vacuum homogenizer, and start the stirring function at a low speed to mix them evenly;

[0046] S2. After step S1 is evenly mixed, initiator MBF, initiator 819, and initiator TPO are added thereto in sequence, and stirred thoroughly until they are completely dissolved;

[0047] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0048] S4: adding GU3300Z and GU3300P, and mixing them evenly after high-speed stirring and dispersion; performing vacuum degassing with the air pressure set to -0.08 MPa for 3 times, each time for 10 minutes, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0049] Example 3

[0050] This embodiment provides a method for preparing a temperature-resistant UV pressure-sensitive adhesive for bonding a notebook frame, comprising the following steps:

[0051] The UV pressure-sensitive adhesive comprises, by weight: 8 parts of ITDA, 7 parts of TBCHA, 18 parts of THFA, 3 parts of initiator MBF, 1 part of initiator TPO, 25 parts of GU3020ZZ, 50 parts of GU8366P, and 3 parts of fumed silica;

[0052] S1. First, add the acrylic acid ester monomers ITDA, TBCHA, and THFA into a vacuum homogenizer according to the above weight, and turn on the stirring function to mix them at a low speed;

[0053] S2. After step S1 is evenly mixed, initiator MBF and initiator TPO are added thereto in sequence, and stirred thoroughly until they are completely dissolved;

[0054] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0055] S4: GU3020ZZ and GU8366P are added, and the mixture is uniformly mixed after high-speed stirring and dispersion; vacuum degassing is performed with the air pressure set to -0.08 MPa, and degassing is performed 3 times, each time for 10 minutes, and then the material is discharged through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0056] Example 4

[0057] This embodiment provides a method for preparing a temperature-resistant UV pressure-sensitive adhesive for bonding a notebook frame, comprising the following steps:

[0058] The UV pressure-sensitive adhesive comprises, by weight: 8 parts of ITDA, 18 parts of TBCHA, 8 parts of THFA, 3 parts of initiator MBF, 0.2 parts of initiator 819, 0.8 parts of initiator TPO, 50 parts of modified acrylate oligomer resin 61217, 30 parts of GU8366P, and 2 parts of fumed silica;

[0059] S1. First, add the acrylic acid ester monomers ITDA, TBCHA, and THFA into a vacuum homogenizer according to the above weight, and start the stirring function at a low speed to mix them evenly;

[0060] S2. After step S1 is evenly mixed, initiator MBF, initiator 819, and initiator TPO are added in sequence, and stirred thoroughly until they are completely dissolved;

[0061] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0062] S4: adding modified acrylic oligomer resin 61217 and GU8366P, and mixing them evenly after high-speed stirring and dispersion; performing vacuum degassing with the air pressure set to -0.08 MPa, and performing degassing for 3 times, each for 10 minutes, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0063] Example 5

[0064] This embodiment provides a method for preparing a temperature-resistant UV pressure-sensitive adhesive for bonding a notebook frame, comprising the following steps:

[0065] The UV pressure-sensitive adhesive comprises, by weight: 10 parts of ITDA, 18 parts of TBCHA, 20 parts of THFA, 3 parts of initiator MBF, 1 part of initiator TPO, 50 parts of modified acrylate oligomer resin 61217, 10 parts of GU8366P, and 4 parts of fumed silica;

[0066] S1. First, add the acrylic acid ester monomers ITDA, TBCHA, and THFA into a vacuum homogenizer according to the above weight, and start the stirring function at a low speed to mix them evenly;

[0067] S2. After step S1 is evenly mixed, initiator MBF and initiator TPO are added thereto in sequence, and stirred thoroughly until they are completely dissolved;

[0068] S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system;

[0069] S4: adding modified acrylic oligomer resin 61217 and GU8366P, and mixing them evenly after high-speed stirring and dispersion; performing vacuum degassing with the air pressure set to -0.08 MPa, and performing degassing for 3 times, each for 10 minutes, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

[0070] Comparative Example 1

[0071] This comparative example is carried out on the basis of the above-mentioned Example 5, and the similarities with the above-mentioned Example are not repeated here.

[0072] In this comparative example, the process is changed. The UV pressure-sensitive adhesive is first cured at 365 nm with a curing energy of 200 mJ / cm 2 Pre-curing is performed, and then the product is laminated. Under the condition of pressure maintenance, the product is subjected to 2000mJ / cm 2 Allow to fully cure.

[0073] Comparative Example 2

[0074] This comparative example is a high-performance pressure-sensitive tape used in the customer's current products.

[0075] The products obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were tested, and the test results are shown in Table 1.

[0076] Table 1

[0077]

[0078] As can be seen from Table 1, from Examples 1, 2 to 3, the initial adhesion is gradually improved, but the improvement of the vertical shear force is not obvious. The cohesive strength of different acrylate oligomers is insufficient, and the bonding ability to the product is insufficient; therefore, at the product bonding application end, the light decay test after 4 hours of high-temperature storage at 60°C shows a decay of more than 12%, far exceeding the target requirement of 5%. The experimental results show that these three groups cannot meet the application; after evaluating other acrylate oligomers, in Example 4, the cohesive strength is improved by the selection of oligomer resin, and the vertical shear strength is also significantly improved. We selected another 2-functional aliphatic polyurethane acrylate oligomer, which will help the initial adhesion to a certain extent; through its experimental test, it has obvious improvement in vertical shear strength, but its weather resistance at high temperature is poor, and it still cannot meet the actual application requirements of the product; Example 5, through the experiment on the oligomer, adjusting its dosage in the formula can effectively improve the weather resistance performance at high temperature.

[0079] The above embodiment is tested according to the following method:

[0080] 1. 90° peel force test method, such as Figure 1 As shown:

[0081] 1. Use SUS stainless steel plate (3) as bonding substrate;

[0082] 2. Glue sample width: 25.0mm, glue sample thickness: 0.25mm (height limit is used when making samples);

[0083] 3. Apply liquid UV pressure-sensitive adhesive (2) through the scraper, and then cure the UV pressure-sensitive adhesive (2) under a 365nm LED light source;

[0084] 4. Curing energy: 4000mJ / cm 2 The cured UV pressure-sensitive adhesive sample was laminated with a 50 μm thick PET original film (1) as the substrate, and a 2 kg roller was used to roll the PET back and forth three times (the process conditions were changed: the liquid UV pressure-sensitive adhesive was scraped through the sample, and then the UV pressure-sensitive adhesive was subjected to 200 mJ / cm under a 365 nm LED light source. 2 Initial curing, the cured UV pressure-sensitive adhesive sample is laminated with a 50μm thick PET original film as the substrate, and the PET is rolled back and forth 3 times with a 2KG roller, and then 2000mJ / cm 2 The energy is fully solidified);

[0085] 5. Standing time: 20min;

[0086] 6. Test speed: 300mm / min;

[0087] 7. Sampling interval: 100mm;

[0088] 8. Test environment: 25±3℃, 50±15%RH (normal temperature); 65±5℃ (high temperature) after 1 hour of storage; -25±5℃ (low temperature) after 1 hour of storage and then tested in the environment;

[0089] 9. Test quantity: 3pcs;

[0090] Second, shear force test method, such as Figure 2 As shown:

[0091] 1. Use SUS stainless steel plate (3) as bonding substrate;

[0092] 2. Glue sample size: 10.0*10.0mm, glue sample thickness: 0.25mm (height limit when making samples);

[0093] 3. Apply liquid UV pressure-sensitive adhesive (2) through the scraper, and then cure the UV pressure-sensitive adhesive under a 365nm LED light source;

[0094] 4. Curing energy: 4000mJ / cm 2 The cured UV pressure-sensitive adhesive sample was laminated with a 50 μm thick PET film (1) as the substrate, and the PET film was rolled back and forth three times using a 2 kg roller (optimized process conditions: the liquid UV pressure-sensitive adhesive was scraped through the sample, and then the UV pressure-sensitive adhesive was exposed to 200 mJ / cm2 of LED light at 365 nm). 2 Pre-curing, the cured UV pressure-sensitive adhesive sample is laminated with a 50μm thick PET film as the substrate, and the PET film is rolled back and forth 3 times with a 2KG roller, and then 2000mJ / cm 2 The energy is fully solidified);

[0095] 5. Test environment: 25±3℃, 50±15%RH (normal temperature); 65±5℃ (high temperature) after 1 hour of storage; -25±5℃ (low temperature) after 1 hour of storage and then tested in the environment;

[0096] 6. Standing time: 20min;

[0097] 7. Test speed: 10mm / min;

[0098] 8. Test quantity: 3pcs.

[0099] In summary, the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding of the present invention is an acrylic acid + UV system pressure-sensitive adhesive, which can have a certain initial adhesion after UV curing, replacing the application of traditional pressure-sensitive tapes; the adhesion and shear force of the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding of the present invention are higher than those of tapes; the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding of the present invention has passed the test and has obvious advantages over the same type of tapes / UV pressure-sensitive adhesives; the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding of the present invention has good cohesion and is not affected by the reworkability of the process.

[0100] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A heat-resistant UV pressure-sensitive adhesive for bonding notebook frames, characterized in that: The total weight of the heat-resistant UV pressure-sensitive adhesive is 115.0-120.0 g, and includes the following components in parts by weight: Modified acrylate oligomer resin: 40-90 parts; Acrylate monomer: 20-60 parts; Initiator: 1-5 parts; Silicon dioxide: 1-5 parts; Wherein, the silicon dioxide is fumed silicon dioxide; the modified acrylate oligomer resin is selected from one or both of a 2-functional polyacrylate oligomer resin or a 2-functional aliphatic polyurethane acrylate oligomer resin.

2. The heat-resistant UV pressure-sensitive adhesive for notebook frame bonding according to claim 1, characterized in that: The 2-functional polyacrylate oligomer resin is selected from one or more of modified acrylate oligomer resin 61363 and modified acrylate oligomer resin 61217.

3. The heat-resistant UV pressure-sensitive adhesive for bonding notebook frames according to claim 1, characterized in that: The 2-functionality aliphatic polyurethane acrylate oligomer resin is selected from one or more of GU3020Z, GU3300Z, GU3300P, and GU8366P.

4. The heat-resistant UV pressure-sensitive adhesive for bonding notebook frames according to claim 1, characterized in that: The acrylic acid ester monomer is selected from one or more of tetrahydrofuran acrylic acid ester monomer, isobornyl acrylate monomer, isotridecyl acrylate monomer, 4-tert-butylcyclohexyl acrylate monomer, 2-ethylhexyl acrylate monomer, and isooctyl acrylate.

5. The heat-resistant UV pressure-sensitive adhesive for bonding notebook frames according to claim 1, characterized in that: The initiator is selected from one or more of initiator methyl benzoylformate, initiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, initiator 184, initiator 754, and initiator 819.

6. The method for preparing the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding according to any one of claims 1 to 5, characterized in that: The steps include: S1. Add 2 to 5 kinds of acrylic acid ester monomers into a stirring device, turn on the stirring function and mix them at a low speed; S2. After step S1 is evenly mixed, add the initiator thereto and stir thoroughly until it is completely dissolved; S3: After the complete dissolution of step S2, add fumed silica thereto, disperse and stir at high speed, and completely disperse the fumed silica into the system; S4: adding 2-functional polyacrylate oligomer resin and 2-functional aliphatic polyurethane acrylate oligomer resin, and mixing them evenly through high-speed stirring and dispersion; performing continuous degassing by vacuum degassing, and then discharging the material through a 200-mesh filter to obtain the heat-resistant UV pressure-sensitive adhesive for notebook frame bonding.

7. The method for preparing a heat-resistant UV pressure-sensitive adhesive for bonding notebook frames according to claim 6, characterized in that: The vacuum degassing pressure is set to -0.08 MPa, and the continuous degassing is performed 2 to 3 times, each time for 10 to 12 minutes.

8. The method for preparing a heat-resistant UV pressure-sensitive adhesive for bonding notebook frames according to claim 6, characterized in that: The stirring device is selected from a vacuum homogenizing mixer or a double planetary mixer.