Easily stripped high-viscosity adhesive tape and preparation method thereof
By pretreating the corona pretreatment of polyethylene terephthalate substrate and combining acrylic pressure-sensitive adhesive layer and antistatic liquid coating, bonding products in the prior art are solved and bonding products in electronic product protection and Cleaning removes balance issues, improves antistatic performance, suitable for electronic product protection and shipment.
Patent Information
- Application Number
- CN202411078351.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
Existing bonding supplies are difficult to achieve a balance between reliable bonding and clean removal during electronics protection and shipment, and are insufficient antistatic properties, resulting in limited application.
Using a corona pretreated polyethylene terephthalate substrate, combined with acrylic pressure-sensitive adhesive layer and antistatic liquid coating, and forming easy-to-peel high-adhesive tape through silicone release agent to optimize adhesion and peel strength while improving antistatic properties.
It achieves a balance between reliable bonding and clean removal of high-adhesive tape in electronic product protection, has good antistatic properties and weather resistance, and has no residual glue after peeling, which is suitable for the protection and shipment of electronic products.
Smart Images

Figure BDA0004983004190000101 
Figure BDA0004983004190000111
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of adhesive products, and particularly relates to an easy-to-peel high-adhesive tape and a preparation method thereof. Background Art
[0002] With the development of society, industrial production is moving towards high-end precision, and people's requirements for products are also increasing, especially in the surface protection of electronic products, especially for glass panels, electronic processing and manufacturing, composite materials, polishing equipment, matte panels, diffusers and mobile phone screens during processing, assembly and transportation. The existing protective film is mainly composed of a substrate and a pressure-sensitive adhesive. Based on the requirements of high cleanliness, pollution-free, self-wetting and antistatic for electronic products, and the commonly used substrates such as polyethylene terephthalate plastic films are polymer materials with excellent electrical insulation properties, the existing technology often modifies the protective film with antistatic properties to give it an application prospect for electronic product protection packaging.
[0003] In the prior art, the preparation of multi-performance adhesive products often adopts a multi-layer composite form to improve its application performance and application range. The invention patent with application number CN202211665674.4 discloses a preparation process of an antistatic tape, including the following steps: S1, substrate preparation: making a substrate film; S2, antistatic liquid preparation: obtaining an antistatic liquid; S3, pressure-sensitive adhesive preparation: obtaining a pressure-sensitive adhesive; S4, antistatic layer addition: antistatic liquid is coated on the surface of the substrate film; S5, pressure-sensitive adhesive layer addition: pressure-sensitive adhesive is coated on the surface of the substrate film; S6, cutting and winding: using a release film for covering, and using a cutting machine to cut according to the required size, the cut tape is wound up, and the wound tape is packaged to obtain an antistatic tape product, which has strong antistatic performance, strong waterproofness, and strong adhesion, but it does not solve the balance between reliable bonding and clean removal performance, and its function is limited when it is used for electronic product protection and shipment.
[0004] In view of this, an easily peelable high-adhesive tape of the present invention is particularly important. Summary of the invention
[0005] In view of the defects of the prior art, the purpose of the present invention is to provide an easy-to-peel high-viscosity tape and a preparation method thereof. The high-viscosity tape provided by the present invention is a tape that strikes a balance between reliable bonding and clean removal, has a good pressure-sensitive adhesive coating state, good exhaust performance, and no residual adhesive after peeling, and has good weather resistance and stable antistatic performance, and is suitable for use in the protection and shipment of electronic products.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] On one hand, the present invention provides an easily peelable high-adhesive tape, the high-adhesive tape comprising a polyethylene terephthalate substrate, an acrylic pressure-sensitive adhesive layer coated on the upper surface of the substrate, a release layer coated on the upper surface of the acrylic pressure-sensitive adhesive layer, and an antistatic liquid coating coated on the lower surface of the substrate;
[0008] Wherein, the polyethylene terephthalate substrate is subjected to corona pretreatment.
[0009] Preferably, the corona pretreatment step is as follows: turn on the corona machine, set the power to 0.4 KV, and the running speed of the polyethylene terephthalate substrate to 10 m / min, to obtain a polyethylene terephthalate substrate that has been subjected to corona pretreatment.
[0010] The applicant found that the surface of the corona-treated substrate produced active groups such as hydroxyl and carboxyl groups that can be cross-linked, and at the same time, the surface of the polyethylene terephthalate produced a microscopic uneven morphology, which enhanced its adhesion to the acrylic pressure-sensitive adhesive and the antistatic liquid through chemical and physical effects, thereby reducing the adhesive retention rate of high-viscosity tape peeling; on the other hand, the performance of the polyethylene terephthalate substrate that has been pre-treated with corona has also been improved to a certain extent in terms of extensibility, and it is not easy to warp.
[0011] In some embodiments of the present invention, the thickness of the easily peelable high-adhesive tape is 50-55 μm.
[0012] Another aspect of the present invention provides a method for preparing an easily peelable high-adhesive tape, comprising the following steps:
[0013] Preferably, the method for preparing the easily peelable high-adhesive tape comprises the following steps:
[0014] 1) coating an acrylic pressure-sensitive adhesive on the upper surface of a polyethylene terephthalate substrate, and drying at 50 to 75° C. for 5 to 20 minutes to form an acrylic pressure-sensitive adhesive layer with a coating thickness of 14 to 16 μm;
[0015] 2) applying the antistatic liquid on the lower surface of the polyethylene terephthalate substrate, and drying at 80 to 120° C. for 30 to 35 minutes to form an antistatic liquid coating with a coating thickness of 12.5 to 13.5 μm;
[0016] 3) coating the silicone release agent on the upper surface of the acrylic pressure-sensitive adhesive layer to obtain a release layer, and cutting the layer with a cutting machine, and then rolling and packaging the layer to obtain the easily peelable high-adhesive tape.
[0017] Preferably, the polyethylene terephthalate substrate has a thickness of 23-25 μm.
[0018] Preferably, the coating thickness of the silicone release agent is 0.5 μm.
[0019] In some embodiments of the present invention, the acrylic pressure-sensitive adhesive comprises the following raw materials in parts by weight: 65-80 parts of soft monomer, 8-12 parts of hard monomer, 2-2.5 parts of cross-linking monomer, 1-2.7 parts of emulsifier, 0.6-1.2 parts of initiator, and 80-150 parts of deionized water.
[0020] In some embodiments of the present invention, the preparation steps of the acrylic pressure-sensitive adhesive are as follows:
[0021] Add soft monomer, hard monomer and cross-linking monomer into the reactor, stir evenly, then add deionized water and emulsifier, heat to 40-70° C. in an inert gas environment, add initiator, stir evenly, heat to 70-90° C., react for 2-6 hours, cool to below 40° C., adjust pH to 7-8, stir evenly to obtain the acrylic pressure-sensitive adhesive.
[0022] Preferably, the preparation steps of the acrylic pressure-sensitive adhesive are as follows:
[0023] Add soft monomer, hard monomer and cross-linking monomer into the reactor, stir evenly, then add deionized water and emulsifier, heat to 55°C in a nitrogen gas environment, add initiator, stir evenly, heat to 80°C, react for 4h, cool to 40°C, adjust pH to 7-8, stir evenly to obtain the acrylic pressure-sensitive adhesive.
[0024] In some embodiments of the present invention, the soft monomer is 2-ethylhexyl acrylate, the hard monomer is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate and methyl methacrylate, and the crosslinking monomer is sodium p-styrene sulfonate.
[0025] Preferably, the emulsifier is emulsifier DNS-86.
[0026] Preferably, the initiator is ammonium persulfate.
[0027] The present application deeply participates in the cross-linking curing process by preferably cross-linking monomers containing carboxyl and hydroxyl functional groups. At this time, the cured structure formed after the acrylic pressure-sensitive adhesive is formed tends to be a more stable spatial network structure; at the same time, under preferred conditions, the monomers of the acrylic pressure-sensitive adhesive are fully cross-linked, the proportion of unsaturated bonds is reduced, the cohesive strength and bulk viscosity of the acrylic pressure-sensitive adhesive are increased, and its good wetting effect on the corona-pretreated polyethylene terephthalate substrate is ensured, the weakening of the wetting effect on the substrate surface due to excessive cross-linking is avoided, the interfacial bonding force is maintained, and the peel strength of the high-viscosity tape is increased.
[0028] In some embodiments of the present invention, the antistatic liquid comprises the following raw materials in parts by weight: 15 to 40 parts of acrylic resin, 0.1 to 3 parts of isocyanate curing agent, 0.5 to 2 parts of leveling agent, 5 to 10 parts of modified silica nanospheres, 20 to 50 parts of antistatic agent, 20 to 40 parts of deionized water and 30 to 70 parts of organic solvent.
[0029] In some embodiments of the present invention, the preparation steps of the antistatic liquid are as follows:
[0030] (1) adding a first silane coupling agent and a second silane coupling agent to a #1 reactor in sequence, heating to 120-150° C. under an inert atmosphere, stirring and reacting for 3-6 hours, and cooling to room temperature after the reaction is completed to obtain a dispersant;
[0031] (2) adding an organic solvent to the #2 reactor, adjusting the pH to a weak acid, then adding a dispersant, stirring and mixing at 40-50° C. for 3-8 hours, then adding silica nanospheres, continuing to raise the temperature to 60-70° C., stirring and reacting for 3-5 hours, and obtaining modified silica nanospheres;
[0032] (3) Add deionized water, an organic solvent, modified silica nanospheres, an acrylic resin, an isocyanate curing agent, a leveling agent and an antistatic agent into the #3 reactor and stir evenly to obtain the antistatic liquid.
[0033] Preferably, the preparation steps of the antistatic liquid are as follows:
[0034] (1) adding the first silane coupling agent and the second silane coupling agent to the reactor #1 in sequence, heating to 135° C. under a nitrogen atmosphere, stirring for reaction for 4.5 hours, and cooling to room temperature after the reaction to obtain a dispersant;
[0035] (2) Add an organic solvent to the #2 reactor, adjust the pH to 5, then add a dispersant, stir and mix at 45°C for 5.5 hours, then add silica nanospheres, continue to heat to 65°C, stir and react for 4 hours, and obtain modified silica nanospheres;
[0036] (3) Add deionized water, an organic solvent, modified silica nanospheres, an acrylic resin, an isocyanate curing agent, a leveling agent and an antistatic agent into the #3 reactor and stir evenly to obtain the antistatic liquid.
[0037] In some embodiments of the present invention, the first silane coupling agent is γ-aminopropyltriethoxysilane, and the second silane coupling agent is γ-glycidyloxypropyltrimethoxysilane, and the molar ratio of the two is 1:(0.8-1.2).
[0038] Preferably, the molar ratio of the γ-aminopropyltriethoxysilane to the γ-glycidyloxypropyltrimethoxysilane is 1:1.
[0039] In some embodiments of the present invention, the mass ratio of the dispersant to the silica nanospheres in step (2) is (0.05-0.2):1.
[0040] Preferably, the mass ratio of the dispersant to the silica nanospheres is 0.13:1.
[0041] Preferably, the amount of the alcohol organic solvent added is 20 to 40 times the total mass of the dispersant and the silica nanospheres.
[0042] Further preferably, the amount of the alcohol organic solvent added is 30 times the total mass of the dispersant and the silica nanospheres.
[0043] More preferably, the alcohol organic solvent is isopropanol.
[0044] Preferably, the antistatic agent is a lithium salt antistatic agent.
[0045] More preferably, the antistatic agent is lithium bis(trifluoromethanesulfonyl)imide.
[0046] Preferably, the isocyanate curing agent is isocyanate.
[0047] Preferably, the leveling agent is a silicone leveling agent.
[0048] Preferably, the organic solvent is at least one of isobutyl alcohol and isopropyl alcohol.
[0049] In the prior art, in order to improve the antistatic property of the tape, the antistatic effect is often achieved by adding functional additives and inorganic fillers. The present application prepares a network-like silane coupling agent dispersant by utilizing the epoxy ring-opening reaction between the epoxy group and the primary amine group between γ-aminopropyl triethoxysilane and γ-glycidyloxypropyl trimethoxysilane. The alkoxy groups at both ends of the dispersant weaken the tendency of the silica nanosphere particles to combine and aggregate due to the presence of a large number of hydroxyl groups, and improve the adhesion of the silica nanospheres to lithium bis(trifluoromethane) xanthamide, forming a more efficient synergistic enhancement pathway, and improving the antistatic effect on the basis of reducing the amount of antistatic agent added. The possible reason is that the modified silica nanospheres form a mesh structure in which the particles are interconnected and evenly distributed in the antistatic liquid, and the antistatic components are enriched and induced to form a more efficient conductive path under the promotion of the dispersant modification.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] (1) The high-viscosity tape provided by the present invention is a high-viscosity tape that strikes a balance between reliable bonding and clean removal, has a good pressure-sensitive adhesive coating state, good air exhaust performance, and no residual adhesive after peeling. It also has good weather resistance and stable antistatic performance, and is suitable for use in the protection and shipment of electronic products.
[0052] (2) The polyethylene terephthalate substrate of the present invention is subjected to corona pretreatment, and active groups such as hydroxyl and carboxyl groups that can be cross-linked are generated on the surface. At the same time, the uneven morphology generated on its microscopic surface enhances the adhesion through chemical and physical effects, thereby reducing the adhesive retention rate of high-viscosity tape after peeling. On the other hand, the extensibility of the substrate that has been subjected to corona pretreatment is improved, and it is not easy to warp.
[0053] (3) In the preparation of the pressure-sensitive adhesive layer, the present invention uses the preferred cross-linking monomers containing carboxyl and hydroxyl functional groups to deeply participate in the cross-linking and curing process. At this time, the cured structure formed after the acrylic pressure-sensitive adhesive is formed tends to be a more stable spatial network structure; at the same time, under the preferred conditions, the monomers of the acrylic pressure-sensitive adhesive are fully cross-linked, the proportion of unsaturated bonds is reduced, the cohesive strength and bulk viscosity of the acrylic pressure-sensitive adhesive are increased, and its good wetting effect on the polyethylene terephthalate substrate pretreated with corona is ensured, and the weakening of the wetting effect on the substrate surface due to excessive cross-linking is avoided, the interfacial bonding force is maintained, and the peel strength of the high-viscosity tape is increased.
[0054] (4) In the preparation of the antistatic liquid coating, the present invention modifies the silica nanospheres by a dispersant and adds them to the antistatic liquid, thereby avoiding the influence of the aggregation behavior of the silica nanospheres on the compatibility and performance of the antistatic liquid, improving the adhesion of the inorganic filler silica nanospheres to lithium bis(trifluoromethane) xanthamide, forming a more efficient synergistic conductive path, and improving the antistatic effect on the basis of reducing the amount of antistatic agent added. DETAILED DESCRIPTION
[0055] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0056] If not otherwise specified, the reagents used below can be easily obtained from commercial companies, wherein the polyethylene terephthalate substrate was purchased from Yihua Dongli, the silicone release agent was purchased from Hubei Xinsihai Chemical Co., Ltd., the acrylic resin was purchased from Shanghai Xinjihua Plastic Co., Ltd., the silica nanospheres were purchased from Degussa (Qingdao) Co., Ltd., the emulsifier DNS-86 was purchased from Qingxin County Hanke Chemical Technology Co., Ltd., and the silicone leveling agent was purchased from Tianjin Ruike Chemical Trading Co., Ltd.
[0057] Preparation Example 1
[0058] In parts by weight, the preparation steps of the first acrylic pressure-sensitive adhesive are as follows:
[0059] Add 72.5 parts of 2-ethylhexyl acrylate, 10 parts of hydroxypropyl acrylate and 2.3 parts of sodium p-styrene sulfonate into the reactor, stir evenly, add 115 parts of deionized water and 1.9 parts of emulsifier DNS-86, heat to 55°C in a nitrogen gas environment, add 0.9 parts of ammonium persulfate, stir evenly, heat to 80°C, react for 4 hours, cool to 40°C, add ammonia water to adjust the pH to 7.5, stir evenly to obtain the first acrylic pressure-sensitive adhesive.
[0060] Preparation Example 2
[0061] In parts by weight, the preparation steps of the second acrylic pressure-sensitive adhesive are as follows:
[0062] Add 65 parts of 2-ethylhexyl acrylate, 8 parts of hydroxypropyl acrylate and 2 parts of sodium p-styrene sulfonate into the reactor, stir evenly, add 80 parts of deionized water and 1 part of emulsifier DNS-86, heat to 55°C in a nitrogen gas environment, add 0.6 parts of ammonium persulfate, stir evenly, heat to 80°C, react for 4 hours, cool to 40°C, add ammonia water to adjust the pH to 7.5, stir evenly to obtain the second acrylic pressure-sensitive adhesive.
[0063] Preparation Example 3
[0064] In parts by weight, the preparation steps of the third acrylic pressure-sensitive adhesive are as follows:
[0065] Add 80 parts of 2-ethylhexyl acrylate, 12 parts of hydroxypropyl acrylate and 2.5 parts of sodium p-styrene sulfonate into the reactor, stir evenly, add 150 parts of deionized water and 2.7 parts of emulsifier DNS-86, heat to 55°C in a nitrogen gas environment, add 1.2 parts of ammonium persulfate, stir evenly, heat to 80°C, react for 4 hours, cool to 40°C, add ammonia water to adjust the pH to 7.5, stir evenly to obtain the third acrylic pressure-sensitive adhesive.
[0066] Preparation Example 4
[0067] The preparation steps of the first antistatic liquid are as follows:
[0068] (1) Add 1 mol of γ-aminopropyltriethoxysilane and 1 mol of γ-glycidyloxypropyltrimethoxysilane in reactor #1, heat to 135° C. under nitrogen atmosphere, stir and react for 4.5 hours, and cool to room temperature after the reaction to obtain a dispersant;
[0069] (2) Add 339 mL of isopropanol to the #2 reactor, adjust the pH to 5, add 1.3 g of dispersant, stir and mix at 45 °C for 5.5 h, add 10 g of silica nanospheres, continue to heat to 65 °C, stir and react for 4 h, and obtain modified silica nanospheres;
[0070] (3) Add 30 mL of deionized water, 50 g of isopropanol, 7.5 g of modified silica nanospheres, 27.5 g of acrylic resin, 1.6 g of isocyanate, 1.3 g of organic silicone leveling agent and 35 g of lithium bis(trifluoromethanesulfonyl)imide into reactor #3 and stir evenly to obtain a first antistatic liquid.
[0071] Preparation Example 5
[0072] The preparation steps of the second antistatic liquid are as follows: the specific implementation steps are the same as those of Preparation Example 4, except that in step (3), 20 mL of deionized water, 30 g of isopropanol, 5 g of modified silica nanospheres, 15 g of acrylic resin, 0.1 g of isocyanate, 0.5 g of silicone leveling agent and 20 g of lithium bis(trifluoromethanesulfonyl)imide are added to the reactor and stirred evenly to obtain the second antistatic liquid.
[0073] Preparation Example 6
[0074] The preparation steps of the third antistatic liquid are as follows: the specific implementation steps are the same as those of Preparation Example 4, except that in step (3), 40 mL of deionized water, 70 g of isopropanol, 10 g of modified silica nanospheres, 40 g of acrylic resin, 3 g of isocyanate, 2 g of silicone leveling agent and 50 g of lithium bis(trifluoromethanesulfonyl)imide are added to the reactor and stirred evenly to obtain the third antistatic liquid.
[0075] Preparation Example 7
[0076] The fourth antistatic liquid is prepared as follows:
[0077] 30 mL of deionized water, 50 g of isopropanol, 7.5 g of modified silica nanospheres, 27.5 g of acrylic resin, 1.6 g of isocyanate, 1.3 g of an organosilicon leveling agent and 35 g of lithium bis(trifluoromethane) xanthamide were added into a reactor and stirred evenly to obtain a fourth antistatic liquid.
[0078] Preparation Example 10
[0079] The preparation steps of the fifth antistatic liquid are the same as those of Preparation Example 4, except that 0.5 g of dispersant and 10 g of silica nanospheres are added in step (2).
[0080] Preparation Example 11
[0081] The preparation steps of the sixth antistatic liquid are the same as those of Preparation Example 4, except that 2.1 g of dispersant and 10 g of silica nanospheres are added in step (2).
[0082] Preparation Example 12
[0083] The preparation steps of the seventh antistatic liquid are as follows: add 30 mL of deionized water, 50 g of isopropanol, 7.5 g of silica nanospheres, 27.5 g of acrylic resin, 1.6 g of isocyanate, 1.3 g of silicone leveling agent and 35 g of lithium bis(trifluoromethane) xanthamide into a reactor, stir evenly, and obtain the seventh antistatic liquid.
[0084] Example 1
[0085] An easily peelable high-viscosity tape, comprising a corona-pretreated polyethylene terephthalate substrate, an acrylic pressure-sensitive adhesive layer coated on the upper surface of the substrate, a release layer coated on the upper surface of the acrylic pressure-sensitive adhesive layer, and an antistatic liquid coating coated on the lower surface of the substrate;
[0086] The steps of corona pretreatment of the polyethylene terephthalate substrate are as follows: turning on the corona machine, setting the power to 0.4 KV, and the running speed of the polyethylene terephthalate substrate to 10 m / min, to obtain a polyethylene terephthalate substrate that has been corona pretreated;
[0087] The method for preparing the easily peelable high-adhesive tape of this embodiment comprises the following steps:
[0088] 1) coating a first acrylic pressure-sensitive adhesive on the upper surface of a corona-pretreated polyethylene terephthalate substrate, and drying at 62.5° C. for 13 min to form an acrylic pressure-sensitive adhesive layer with a coating thickness of 15 μm;
[0089] 2) coating the first antistatic liquid on the lower surface of the polyethylene terephthalate substrate, and drying at 100° C. for 33 min to form an antistatic liquid coating with a coating thickness of 13 μm;
[0090] 3) coating the silicone release agent on the upper surface of the acrylic pressure-sensitive adhesive layer to obtain a release layer, and cutting the layer using a cutting machine, and then rolling and packaging the layer to obtain the easily peelable high-adhesive tape;
[0091] The polyethylene terephthalate substrate has a thickness of 24 μm, and the coating thickness of the silicone release agent is 0.5 μm.
[0092] Example 2
[0093] An easily peelable high-viscosity tape, comprising a corona-pretreated polyethylene terephthalate substrate, an acrylic pressure-sensitive adhesive layer coated on the upper surface of the substrate, a release layer coated on the upper surface of the acrylic pressure-sensitive adhesive layer, and an antistatic liquid coating coated on the lower surface of the substrate;
[0094] The steps of corona pretreatment of the polyethylene terephthalate substrate are the same as those in Example 1;
[0095] The method for preparing the easily peelable high-adhesive tape of this embodiment comprises the following steps:
[0096] 1) coating a second acrylic pressure-sensitive adhesive on the upper surface of the corona-pretreated polyethylene terephthalate substrate, and drying at 50° C. for 20 min to form an acrylic pressure-sensitive adhesive layer with a coating thickness of 14 μm;
[0097] 2) coating the first antistatic liquid on the lower surface of the polyethylene terephthalate substrate, and drying at 80° C. for 35 min to form an antistatic liquid coating with a coating thickness of 12.5 μm;
[0098] 3) coating the silicone release agent on the upper surface of the acrylic pressure-sensitive adhesive layer to obtain a release layer, and cutting the layer using a cutting machine, and then rolling and packaging the layer to obtain the easily peelable high-adhesive tape;
[0099] The polyethylene terephthalate substrate has a thickness of 23 μm, and the coating thickness of the silicone release agent is 0.5 μm.
[0100] Example 3
[0101] An easily peelable high-viscosity tape, comprising a corona-pretreated polyethylene terephthalate substrate, an acrylic pressure-sensitive adhesive layer coated on the upper surface of the substrate, a release layer coated on the upper surface of the acrylic pressure-sensitive adhesive layer, and an antistatic liquid coating coated on the lower surface of the substrate;
[0102] The steps of corona pretreatment of the polyethylene terephthalate substrate are the same as those in Example 1;
[0103] The method for preparing the easily peelable high-adhesive tape of this embodiment comprises the following steps:
[0104] 1) coating a third acrylic pressure-sensitive adhesive on the upper surface of the corona-pretreated polyethylene terephthalate substrate to form an acrylic pressure-sensitive adhesive layer with a coating thickness of 16 μm;
[0105] 2) coating the first antistatic liquid on the lower surface of the polyethylene terephthalate substrate, and drying at 75° C. for 5 min to form an antistatic liquid coating with a coating thickness of 13.5 μm;
[0106] 3) applying a silicone release agent on the upper surface of the acrylic pressure-sensitive adhesive layer to obtain a release layer, drying at 120° C. for 30 min, and cutting the layer using a cutting machine, and then rolling and packaging the layer to obtain the easily peelable high-adhesive tape;
[0107] The polyethylene terephthalate substrate has a thickness of 25 μm, and the coating thickness of the silicone release agent is 0.5 μm.
[0108] Example 4
[0109] An easily peelable high-adhesive tape and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is a second antistatic liquid.
[0110] Example 5
[0111] An easily peelable high-adhesive tape and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is a third antistatic liquid.
[0112] Example 6
[0113] An easily peelable high-adhesive tape and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is a fourth antistatic liquid.
[0114] Example 7
[0115] An easily peelable high-adhesive tape and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is the fifth antistatic liquid.
[0116] Example 8
[0117] An easily peelable high-adhesive tape and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is the sixth antistatic liquid.
[0118] Example 9
[0119] An easily peelable high-adhesive tape and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the antistatic liquid coated on the lower surface of the substrate is the seventh antistatic liquid.
[0120] Comparative Example 1
[0121] An easily peelable high-adhesive tape and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the polyethylene terephthalate substrate is not subjected to corona pretreatment.
[0122] Performance Test:
[0123] (1) Initial tack test: The initial tack performance test of the high-viscosity tapes prepared in each embodiment and comparative example was conducted according to the standard GB / T4852-2002 "Test method for initial tack of pressure-sensitive adhesive tapes (rolling ball method)", and the initial tack force rolling ball was required to be greater than 9#;
[0124] (2) Peel strength test: A 180° peel strength test of the high-viscosity tapes prepared in each embodiment and comparative example was performed at a peeling speed of 300 mm / min according to the standard GB / T2792-2014 using a BLD-200S electronic glass testing machine;
[0125] (3) Water resistance test: The high-viscosity tapes prepared in each embodiment and comparative example were immersed in 50° C. water for 24 hours and then the state of the high-viscosity tapes was observed to see if they fell off;
[0126] (4) Antistatic performance test: The volume resistivity of the high-viscosity tape prepared in each embodiment and comparative example was tested according to standard GB / T 31838.2-2019. The smaller the resistance, the better the antistatic performance.
[0127] Table 1
[0128]
[0129]
[0130] As can be seen from Table 1, the high-viscosity tape prepared in Examples 1 to 5 of the present invention is a high-viscosity tape that strikes a balance between reliable bonding and clean removal, has a good pressure-sensitive adhesive coating state, good air exhaust performance, and no residual adhesive after peeling, and has good water resistance and stable antistatic performance; as can be seen from the comparison of Examples 6-9, the modification conditions of the modified silica nanospheres are changed, which mainly affects the performance of the antistatic liquid, has a certain impact on the initial adhesion and peel strength of the high-viscosity tape, and the antistatic performance is greatly reduced due to the poor compatibility of the system. Affected by the bonding effect, the water resistance of the high-viscosity tape is also deteriorated, especially the high-viscosity tape prepared in Example 6 falls off; By comparing Examples 1 to 5 and Comparative Example 1, it can be seen that the polyethylene terephthalate substrate directly used has poor adhesion to the upper and lower adhesive layers, resulting in poor peel strength of the high-viscosity tape, and reduced water resistance and antistatic performance.
[0131] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. An easy-to-peel high-adhesive tape. It is characterized in that The high-viscosity tape comprises a polyethylene terephthalate substrate, an acrylic pressure-sensitive adhesive layer coated on the upper surface of the substrate, a release layer coated on the upper surface of the acrylic pressure-sensitive adhesive layer, and an antistatic liquid coating coated on the lower surface of the substrate; Wherein, the polyethylene terephthalate substrate is subjected to corona pretreatment.
2. The easily peelable high-adhesive tape according to claim 1, It is characterized in that The thickness of the easily peelable high-adhesive tape is 50-55 μm.
3. A method for preparing the easily peelable high-adhesive tape according to any one of claims 1 to 2, It is characterized in that The following steps are involved: 1) coating an acrylic pressure-sensitive adhesive on the upper surface of a polyethylene terephthalate substrate, and drying at 50 to 75° C. for 5 to 20 minutes to form an acrylic pressure-sensitive adhesive layer with a coating thickness of 14 to 16 μm; 2) applying the antistatic liquid on the lower surface of the polyethylene terephthalate substrate, and drying at 80 to 120° C. for 30 to 35 minutes to form an antistatic liquid coating with a coating thickness of 12.5 to 13.5 μm; 3) coating the silicone release agent on the upper surface of the acrylic pressure-sensitive adhesive layer to obtain a release layer, and cutting the layer with a cutting machine, winding the layer, and packaging the layer to obtain the easily peelable high-adhesive tape.
4. The method for preparing the easily peelable high-adhesive tape according to claim 3, It is characterized in that The acrylic pressure-sensitive adhesive comprises the following raw materials in parts by weight: 65-80 parts of soft monomer, 8-12 parts of hard monomer, 2-2.5 parts of cross-linking monomer, 1-2.7 parts of emulsifier, 0.6-1.2 parts of initiator and 80-150 parts of deionized water.
5. The method for preparing the easily peelable high-adhesive tape according to claim 4, It is characterized in that The preparation steps of the acrylic pressure-sensitive adhesive are as follows: Add soft monomer, hard monomer and cross-linking monomer into the reactor, stir evenly, then add deionized water and emulsifier, heat to 40-70° C. in an inert gas environment, add initiator, stir evenly, heat to 70-90° C., react for 2-6 hours, cool to below 40° C., adjust pH to 7-8, stir evenly to obtain the acrylic pressure-sensitive adhesive.
6. The method for preparing the easily peelable high-adhesive tape according to claim 5, It is characterized in that The soft monomer is 2-ethylhexyl acrylate, the hard monomer is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate and methyl methacrylate, and the cross-linking monomer is sodium p-styrene sulfonate.
7. The method for preparing the easily peelable high-adhesive tape according to claim 3, It is characterized in that The antistatic liquid comprises the following raw materials in parts by weight: 10 to 30 parts of acrylic resin, 0.1 to 3 parts of isocyanate curing agent, 1 to 3 parts of leveling agent, 5 to 10 parts of modified silicon dioxide nanospheres, 20 to 50 parts of antistatic agent, 20 to 40 parts of deionized water and 100 to 150 parts of organic solvent.
8. The method for preparing the easily peelable high-adhesive tape according to claim 7, It is characterized in that The preparation steps of the antistatic liquid are as follows: (1) Preparation of modified silica nanospheres: In reactor #1, add a first silane coupling agent and a second silane coupling agent in sequence, heat to 120-150°C under an inert atmosphere, stir and react for 3-6 hours, and cool to room temperature after the reaction to obtain a dispersant; in reactor #2, add an alcohol organic solvent, adjust the pH to a weak acid, then add a dispersant, stir and mix at 40-50°C for 3-8 hours, then add silica nanospheres, continue to heat to 60-70°C, stir and react for 3-5 hours, and obtain modified silica nanospheres; (3) Add deionized water, an organic solvent, modified silica nanospheres, an acrylic resin, an isocyanate curing agent, a leveling agent and an antistatic agent into the #3 reactor and stir evenly to obtain the antistatic liquid.
9. The method for preparing the easily peelable high-adhesive tape according to claim 8, It is characterized in that The first silane coupling agent is γ-aminopropyltriethoxysilane, and the second silane coupling agent is γ-glycidyloxypropyltrimethoxysilane, and the molar ratio of the two is 1:(0.8-1.2).
10. The method for preparing the easily peelable high-adhesive tape according to claim 8, It is characterized in that The mass ratio of the dispersant to the silicon dioxide nanospheres is (0.05-0.2):1.
Citation Information
Cited By
Preparation process of ethylene propylene rubber base material for insulating waterproof adhesive tape
CN119639362A
Preparation process of ethylene-propylene rubber base material for insulating waterproof adhesive tape
CN119639362B